A short glass fiber, stone paper technology, applied in chemical instruments and methods, glass/slag layered products, layered products, etc., can solve the limitations of stone paper promotion and application, folding and tear resistance, stiffness, stiffness, etc. Poor physical properties, etc., to achieve the effect of improving stiffness, good processing performance, and improving folding resistance and tear resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0044] formula:
[0045] The masterbatch formula of the upper surface layer, by mass percentage:
[0046] CaCO 3 40%
[0047] PP (homopolymer) 55%
[0048] Titanate coupling agent 1%
[0049] Polypropylene Wax Dispersant 1%
[0050] Flame retardant 1%
[0051] Compatibilizer 1%
[0052] Slip agent 1%
[0053] The masterbatch formula of the middle layer, by mass percentage:
[0054] Short glass fiber 27%
[0055] PP (homopolymer) 50%
[0056] Hollow glass microspheres 20%;
[0057] Silicate coupling agent 0.5%
[0058] Polypropylene wax dispersant 0.5%
[0059] Flame retardant 1%
[0060] Compatibilizer 0.5%
[0061] Slip agent 0.5%
[0062] The masterbatch formula of the lower surface layer, by mass percentage:
[0063] CaCO 3 60%
[0064] PP (homopolymer) 37%
[0065] Titanate coupling agent 0.5%
[0066] Polypropylene wax dispersant 0.5%
[0067] Flame retardant 1%
[0068] ...
Embodiment 2
[0076] formula:
[0077] The masterbatch formula of the upper surface layer, by mass percentage:
[0078] CaCO 3 50%
[0079] PP (homopolymer) 47.2%
[0080] Titanate coupling agent 0.8%
[0081] Polypropylene wax dispersant 0.5%
[0082] Flame retardant 0.5%
[0083] Compatibilizer 0.5%
[0084] Slip agent 0.5%
[0085] The masterbatch formula of the middle layer, by mass percentage:
[0086] Short glass fiber 25%
[0087] PP (homopolymer) 47.2%
[0088] Hollow glass microspheres 25%;
[0089] Silicate coupling agent 0.8%
[0090] Polypropylene wax dispersant 0.5%
[0091] Flame retardant 0.5%
[0092] Compatibilizer 0.5%
[0093] Slip agent 0.5%
[0094] The masterbatch formula of the lower surface layer, by mass percentage:
[0095] CaCO 3 50%
[0096] PP (homopolymer) 47.2%
[0097] Titanate coupling agent 0.8%
[0098] Polypropylene wax dispersant 0.5%
[0099] Flame ret...
Embodiment 3
[0108] formula:
[0109] The masterbatch formula of the upper surface layer, by mass percentage:
[0110] CaCO 3 60%
[0111] PP (homopolymer) 37%
[0112] Titanate coupling agent 0.5%
[0113] Polypropylene wax dispersant 0.5%
[0114] Flame retardant 1%
[0115] Compatibilizer 0.5%
[0116] Slip agent 0.5%
[0117] The masterbatch formula of the middle layer, by mass percentage:
[0118] Short glass fiber 30%
[0119] PP (homopolymer) 35%
[0120] Hollow glass microspheres 30%;
[0121] Silicate coupling agent 1%
[0122] Polypropylene Wax Dispersant 1%
[0123] Flame retardant 1%
[0124] Compatibilizer 1%
[0125] Slip agent 1%
[0126] The masterbatch formula of the lower surface layer, by mass percentage:
[0127] CaCO 3 40%
[0128] PP (homopolymer) 55%
[0129] Titanate coupling agent 1%
[0130] Polypropylene Wax Dispersant 1%
[0131] Flame retardant 1%
[0132] ...
PUM
| Property | Measurement | Unit |
|---|---|---|
| thickness | aaaaa | aaaaa |
| thickness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More