Composite board made of waste plastic and phosphorus slag fine powder and production method thereof
A technology for waste plastics and composite boards, applied in the field of building materials, can solve problems such as excessive resource occupation, and achieve the effects of reducing pollution, light weight and good market prospects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] Composite boards are made in the following steps:
[0025] a. 400Kg of waste polypropylene and 200Kg of waste polyethylene plastics are sorted and cleaned, crushed to less than 20mm, and mixed uniformly to obtain product A.
[0026] b. Send product A to the feed port of the screw extruder through the conveyor belt, at a screw speed of 35r / min and a barrel temperature of 190 0 Under C condition, carry out the first segment of screw extrusion to obtain B product.
[0027] c. Mix 100Kg phosphorus slag fine powder with product B through the feed port, screw speed 25r / min, barrel temperature 150 0 Under C condition, carry out the second section of screw extrusion to obtain C product.
[0028] d. After calendering product C under a pressure condition of 3.5Mpa by a sheeting roller and two cooling rollers, the finished product is obtained by heating and leveling, cooling by arranging rollers, and trimming and shearing.
Embodiment 2
[0030] Composite boards are made in the following steps:
[0031] a. 500Kg of waste polypropylene and 250Kg of waste polyethylene plastics are sorted and cleaned, crushed to less than 20mm, and mixed uniformly to obtain product A.
[0032] b. Send product A to the feed port of the screw extruder through the conveyor belt, at a screw speed of 35r / min and a barrel temperature of 190 0 Under C condition, carry out the first segment of screw extrusion to obtain B product.
[0033] c. Mix 250Kg phosphorus slag fine powder with product B through the feed port, screw speed 25r / min, barrel temperature 150 0 Under C condition, carry out the second section of screw extrusion to obtain C product.
[0034] d. After calendering product C under a pressure condition of 3.5Mpa by a sheeting roller and two cooling rollers, the finished product is obtained by heating and leveling, cooling by arranging rollers, and trimming and shearing.
Embodiment 3
[0036] Composite boards are made in the following steps:
[0037] a. After sorting and cleaning 700Kg of waste polypropylene and 400Kg of waste polyethylene plastics, they are crushed to less than 20mm, and mixed uniformly to obtain product A.
[0038] b. Send product A to the feed port of the screw extruder through the conveyor belt, at a screw speed of 35r / min and a barrel temperature of 190 0 Under C condition, carry out the first segment of screw extrusion to obtain B product.
[0039] c. Mix 400Kg phosphorus slag fine powder with product B through the feed port, screw speed 25r / min, barrel temperature 150 0 Under C condition, carry out the second section of screw extrusion to obtain C product.
[0040] d. After calendering product C under a pressure condition of 3.5Mpa by a sheeting roller and two cooling rollers, the finished product is obtained by heating and leveling, cooling by arranging rollers, and trimming and shearing.