Embodiment 1
[0054] The raw ore composition of vanadium-bearing stone coal is V 2 o 5 1.4%, K + 0.66%, Fe 总 1.04%, Al 2 o 3 3.75%, Si 2 O81%, C8.75%, and the balance is impurities. Its bulk density is 0.95g / cm 3 , the true density is 1.12g / cm 3 .
[0055] The raw ore is processed with a jaw crusher, and the particle size of the raw ore after processing is up to 5mm. Take 500kg and add 100kg of sulfuric acid with a mass concentration of 93% and 50L of tap water to mix evenly with a concrete mixer, then store the mixture on the thermal insulation material, cover the thermal insulation material in the pile, and store it for 80 hours.
[0056] The stockpiled ore is crushed manually to ensure that the maximum particle size of the ore is less than 10cm. Take 200kg of mixed ore and add 200L of water, mechanically stir in the leaching tank for 1.0h, and filter the output filtrate to 152.5L, containing 11.5g / L of vanadium pentoxide, vanadium The leaching rate was 89.5%.
[0057] The leac...
Embodiment 2
[0062] The raw ore composition of vanadium-bearing stone coal is V 2 o 5 1.9%, K + 0.65%, Fe 总 1.02%, Al 2 o 3 3.7%, Si 2 O81%, C8.8%, and the rest are impurities. Its bulk density is 0.97g / cm 3 , the true density is 1.12g / cm 3 .
[0063] The raw ore is processed with a jaw crusher, the particle size of the raw ore is less than 5mm, and then ball milled, and the slag with a particle size of ore powder less than 0.074mm is 45%. Take 400kg and add 800kg of sulfuric acid with a mass concentration of 95% and 40L of tap water to mix evenly with a concrete mixer, and then store the mixture on the thermal insulation material.
[0064] The stockpile ore is broken manually to ensure that the maximum particle size of the ore is less than 10cm. Take 200kg of mixed ore and add 200L of leaching slag washing water, mechanically stir in the leaching tank for 1.0h, and filter the output filtrate 153.8L, containing 12.5g / L, vanadium leaching rate is 91.5%.
[0065] The leaching sol...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |
| density | aaaaa | aaaaa |