A method for smelting brown corundum by using dust removal powder

A technology of dust removal powder and brown corundum, which is applied in the field of smelting brown corundum, can solve the problems of increasing the production cost of enterprises, the impact of dust removal powder on environmental protection, and high procurement costs, so as to ensure stability, solve the waste of dust removal powder and environmental protection, and reduce production costs. Effect

Active Publication Date: 2017-07-14
YICHUAN DONGFENG ABRASIVES
View PDF0 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] As we all know, brown corundum is a brown artificial corundum made of bauxite, iron filings and coke as the main raw materials, and is smelted at high temperature in an electric arc furnace. Because of its good toughness, high melting point, corrosion resistance and linear expansion Because of its low coefficient and good grinding performance, brown corundum is often selected to be crushed, screened and prepared, and then made into metals suitable for processing and grinding with high tensile strength, such as various general steels, malleable cast irons, carbon steels and hardened At the same time, brown corundum can also be used to manufacture high-grade refractory materials; on the other hand, brown corundum dust removal powder, commonly known as dust collection powder, refers to the ultrafine dust collected during the brown corundum crushing process. This substance is quite different from the finished products of brown corundum smelting, so it is often piled up as waste by brown corundum processing enterprises; Powder will not only affect environmental protection, but also cause serious waste of resources, and correspondingly increase the production cost of the enterprise. Therefore, how to reduce the fine particle size and large impurities. The application of dedusting powder of titanium dioxide and coke powder in the production of brown corundum has become one of the important research topics in brown corundum smelting.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

example 1

[0026] A. According to the weight ratio, add 1 part of 200-mesh dedusting powder into a container with 2 parts of 90 degrees hot water, and stir fully to make the slurry uniform and then place it for 5 hours;

[0027] B. Add 4 parts of aluminum oxide powder into the container, and fully stir evenly, and then use a filter press to dehydrate the slurry to form a granular material with a diameter of 20mm;

[0028] C. Use the secondary waste heat of the smelting furnace to dry and roast the granular material to completely dehydrate the granular material, and then send the granular material to the mixing bin;

[0029] D. Add 0.04 parts of precipitant iron filings and 0.02 parts of coke as reducing agent into the mixing bin, and mix well;

[0030] E. Use the feeder to feed the mixed materials into the electric arc smelting furnace, and carry out layer-by-layer feeding reaction smelting and refining through the electric arc smelting furnace, and finally produce brown corundum after i...

example 2

[0032] A. According to the weight ratio, add 1 part of 325-mesh dedusting powder into a container with 6 parts of 85 degrees of hot water, and stir fully to make the slurry uniform and place it for 6 hours;

[0033] B. Add 15 parts of aluminum oxide powder to the container, and fully stir evenly, and then use a filter press to dehydrate the slurry to form a granular material with a diameter of 20mm;

[0034] C. Use the secondary waste heat of the smelting furnace to dry and roast the granular material to completely dehydrate the granular material, and then send the granular material to the mixing bin;

[0035] D. Add 0.02 parts of iron filings as a precipitant and 0.012 parts of coke as a reducing agent into the mixing bin, and mix well;

[0036] E. Use the feeder to feed the mixed materials into the electric arc smelting furnace, and carry out layer-by-layer feeding reaction smelting and refining through the electric arc smelting furnace, and finally produce brown corundum af...

example 3

[0038] A. According to the weight ratio, add 1 part of 325-mesh dust removal powder into a container with 6 parts of 85 degrees of hot water, and stir fully to make the slurry uniform and then place it for 5.5 hours;

[0039] B. Add 15 parts of aluminum oxide powder to the container, and fully stir evenly, and then use a filter press to dehydrate the slurry to form a 20mm granular material;

[0040] C. Use the secondary waste heat of the smelting furnace to dry and roast the granular material to completely dehydrate the granular material, and then send the granular material to the mixing bin;

[0041] D. Add 0.026 parts of iron filings as a precipitant and 0.015 parts of coke as a reducing agent into the mixing bin, and mix well;

[0042] E. Use the feeder to feed the mixed materials into the electric arc smelting furnace, and carry out layer-by-layer feeding reaction smelting and refining through the electric arc smelting furnace, and finally produce brown corundum after insp...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
Diameteraaaaaaaaaa
Login to View More

Abstract

A method for smelting brown corundum by using dedusting powder, which relates to the field of smelting brown corundum. The method uses adding dedusting powder into hot water, stirring evenly with alumina powder to produce granular materials, and then dehydrating the dehydrated granular materials Send it to the mixing bin to mix evenly with coke and iron filings, and finally pass through the electric arc smelting furnace for layer-by-layer feeding reaction smelting and refining, and after inspection, cooling, grading, crushing and screening, the finished product of brown corundum is obtained; The above method can effectively use dust removal powder to produce smelted brown corundum, which not only reduces the production cost of the enterprise, but also solves the environmental protection problem of corundum correspondingly.

Description

[0001] 【Technical field】 [0002] The invention relates to the field of brown corundum smelting, in particular to a method for smelting brown corundum by using discarded brown corundum dedusting powder. [0003] 【Background technique】 [0004] As we all know, brown corundum is a brown artificial corundum made of bauxite, iron filings and coke as the main raw materials, and is smelted at high temperature in an electric arc furnace. Because of its good toughness, high melting point, corrosion resistance and linear expansion Because of its low coefficient and good grinding performance, brown corundum is often selected to be crushed, screened and prepared, and then made into metals suitable for processing and grinding with high tensile strength, such as various general steels, malleable cast irons, carbon steels and hardened At the same time, brown corundum can also be used to manufacture high-grade refractory materials; on the other hand, brown corundum dust removal powder, common...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine