Healthy and environment-friendly building inner wall coating
A technology for building interiors and coatings, applied in antifouling/underwater coatings, polyurea/polyurethane coatings, coatings, etc., can solve the problems of not being able to improve the indoor environment, achieve indoor air improvement, excellent photocatalytic performance, and enhance degradation efficiency effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] Prepare paint as follows:
[0029] (1) crushing and grinding the adsorbent, and screening to obtain adsorbent particles with a particle size of 0.1-10 microns;
[0030] (2) Mix 1 part of the adsorbent particles described in (1) with 20 parts of titanium dioxide nanopowder according to the required mass fraction;
[0031] (3) Under the condition of less than 500r / min, mix 0.2 part of dispersant, 0.1 part of defoamer and 0.1 part of wetting agent evenly;
[0032] (4) Under the condition of 500-1000r / min, add 21 parts of the mixture of adsorbent particles and titanium dioxide nanopowder, 20 parts of filler, 5 parts of air microcapsules and plant fiber to the above-mentioned dispersant, defoamer and wetting agent mixture 1 part and mix well;
[0033] (5) Under the condition of less than 500r / min, add 40 parts of aqueous emulsion and 1 part of film-forming aid to the mixture (4) and mix well.
Embodiment 2
[0035] Prepare paint as follows:
[0036] (1) crushing and grinding the adsorbent, and screening to obtain adsorbent particles with a particle size of 0.1-10 microns;
[0037] (2) Mix 5 parts of the adsorbent particles described in (1) with 25 parts of titanium dioxide nanopowder according to the required mass fraction;
[0038] (3) Under the condition of less than 500r / min, mix 0.5 part of dispersant, 0.2 part of defoamer and 0.1 part of wetting agent evenly;
[0039] (4) Under the condition of 500-1000r / min, add 21 parts of the mixture of adsorbent particles and titanium dioxide nanopowder, 15 parts of filler, 15 parts of air microcapsules and plant fiber to the above-mentioned dispersant, defoamer and wetting agent mixture 5 parts and mix well;
[0040] (5) Under the condition of less than 500r / min, add 60 parts of aqueous emulsion and 2.5 parts of film-forming aid to the mixture (4) and mix well.
Embodiment 3
[0042] (1) crushing and grinding the adsorbent, and screening to obtain adsorbent particles with a particle size of 0.1-10 microns;
[0043] (2) Mix 2.5 parts of the adsorbent particles described in (1) with 30 parts of titanium dioxide nanopowder according to the required mass fraction;
[0044] (3) Under the condition of less than 500r / min, mix 0.8 part of dispersant, 0.2 part of defoamer and 0.2 part of wetting agent evenly;
[0045] (4) Under the condition of 500-1000r / min, add 32.5 parts of the mixture of adsorbent particles and titanium dioxide nanopowder, 20 parts of filler, 25 parts of air microcapsules and plant fiber to the above-mentioned mixture of dispersant, defoamer and wetting agent 3 parts and mix well;
[0046] (5) Under the condition of less than 500r / min, add 60 parts of aqueous emulsion and 5 parts of film-forming aid to the mixture (4) and mix well.
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction