Making method for glassine paper
A glassine paper and paper technology, applied in the field of papermaking, can solve the problems of poor oil resistance and low surface intermolecular tension, and achieve the effects of good tightness, improved gloss and good transparency
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0020] A preparation method for glassine paper, comprising the following steps:
[0021] (1) Making base paper;
[0022] (2) Coating wetting: Use a humidifier to adjust the humidity, install a heating device in the humidifier system, use hot water for wetting, and control the temperature of the hot water at 30°C to control the moisture content of the paper so that the moisture content of the paper Reach 20%, stop wetting; A heating system is installed on the calender, and the heating system is provided with a steam flow meter, a temperature gauge and a pressure gauge;
[0023] (3) storage;
[0024] (4) Overpressure: use a calender for calendering, and the calender is equipped with at least 3 calendering zones, and the pressure is 1000KN / m 2 , the temperature is 180°C;
[0025] (5) Storage and heat dissipation;
[0026] (6) Rewinding;
[0027] (7) Pack and store.
Embodiment 2
[0029] A preparation method for glassine paper, comprising the following steps:
[0030] (1) Making base paper;
[0031] (2) Coating wetting: use a humidifier to adjust the humidity, install a heating device in the humidifier system, use hot water for wetting, and control the temperature of the hot water at 60°C to control the moisture content of the paper so that the moisture content of the paper Reach 21%, stop wetting; The calender is equipped with a heating system, and the heating system is provided with a steam flow meter, a thermometer and a pressure gauge;
[0032] (3) storage;
[0033] (4) Overpressure: use a calender for calendering. The calender is equipped with at least 3 calendering zones, and the pressure is 1100KN / m 2 , the temperature is 200°C;
[0034] (5) Storage and heat dissipation;
[0035] (6) Rewinding;
[0036] (7) Pack and store.
Embodiment 3
[0038] A preparation method for glassine paper, comprising the following steps:
[0039] (1) Making base paper;
[0040] (2) Coating wetting: Use a humidifier to adjust the humidity, install a heating device in the humidifier system, use hot water for wetting, and control the temperature of the hot water at 90°C to control the moisture content of the paper so that the moisture content of the paper Reach 21%, stop wetting; The calender is equipped with a heating system, and the heating system is provided with a steam flow meter, a thermometer and a pressure gauge;
[0041] (3) storage;
[0042] (4) Overpressure: use a calender for calendering, and the calender is equipped with at least 3 calendering zones, and the pressure is 1200KN / m 2 , the temperature is 220°C;
[0043] (5) Storage and heat dissipation;
[0044] (6) Rewinding;
[0045] (7) Pack and store.
[0046] In the preparation method of glassine paper of the present invention, the paper is conditioned by a humidi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com