A Method for Preventing Cracking and Deformation of Poplar
A cracking and deformation, poplar technology, applied in the direction of humidity control wood, impregnated wood, wood impregnation, etc., can solve the problems of poplar furniture prone to cracking and deformation, environmental and human damage, and inadequate drying, so as to maintain natural Color, avoid cracking and deformation, easy to remove effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A method for preventing cracking and deformation of poplar, comprising the following steps:
[0019] (1) Poplar wetting: Wet fresh poplar before peeling. The temperature is 10°C and the ambient humidity is 84%. Based on the weight of poplar, the amount of wetting liquid sprayed is 50ml / kg, and the wetting liquid is sprayed twice a day. , until the water content of the bark is 75-80%, so that the water content of the poplar is uniform, and when it is wet, it will have a poplar bark, which will give full play to the protective effect of the poplar bark, prevent the poplar from swelling, and make the fiber structure of the poplar wood even and dense after absorbing water. to moisten poplar;
[0020] (2) Freeze-drying of poplar wood: freeze-dry the wet poplar wood at -42°C until the water content is 20-22%, quickly remove the moisture in the poplar wood, make the pores between the poplar wood fibers more fine and uniform, increase the air permeability, It can be quickly lo...
Embodiment 2
[0030] A method for preventing cracking and deformation of poplar, comprising the following steps:
[0031] (1) Poplar wetting: Wet fresh poplar before peeling. The temperature is 11°C and the ambient humidity is 85%. According to the weight of poplar, the amount of wetting liquid sprayed is 55ml / kg, and the wetting liquid is sprayed twice a day. , until the water content of the bark is 75-80%, so that the water content of the poplar is uniform, and when it is wet, it will have a poplar bark, which will give full play to the protective effect of the poplar bark, prevent the poplar from swelling, and make the fiber structure of the poplar wood even and dense after absorbing water. to moisten poplar;
[0032] (2) Freeze-drying of poplar wood: freeze-dry the wet poplar wood at -41°C until the water content is 20-22%, quickly remove the moisture in the poplar wood, make the pores between the poplar wood fibers more fine and uniform, increase the air permeability, It can be quickl...
Embodiment 3
[0042] A method for preventing cracking and deformation of poplar, comprising the following steps:
[0043] (1) Poplar wetting: Wet fresh poplar before peeling. The temperature is 12°C and the ambient humidity is 86%. According to the weight of poplar, the amount of wetting liquid sprayed is 60ml / kg, and the wetting liquid is sprayed 3 times a day. , until the water content of the bark is 75-80%, so that the water content of the poplar is uniform, and when it is wet, it will have a poplar bark, which will give full play to the protective effect of the poplar bark, prevent the poplar from swelling, and make the fiber structure of the poplar wood even and dense after absorbing water. to moisten poplar;
[0044] (2) Freeze-drying of poplar wood: freeze-dry the wet poplar wood at -40°C until the water content is 20-22%, quickly remove the moisture in the poplar wood, make the pores between the poplar wood fibers more fine and uniform, increase the air permeability, It can be quic...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com