Nano-silver complex solution and preparation method thereof
A technology of nano-silver and nano-silver powder is applied in the fields of botanical equipment and methods, chemicals for biological control, food preservation, etc., and can solve problems such as unfavorable popularization and use.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0033] (1) 1g of nano-silver powder is added to 100ml of 1.5wt% PVP aqueous solution, and ultrasonically stirred for 1h to obtain a suspension of nano-silver;
[0034] (2) 8g sodium persulfate is added to 350ml deionized water, stirred and dissolved to obtain sodium persulfate solution;
[0035] (3) Add the sodium persulfate solution described in step (2) into a 1L flask, heat in a water bath (35°C), then add the nano-silver suspension solution described in step (1) to the sodium persulfate solution, and continue the water bath Heating and stirring for 24 hours to obtain a complex solution;
[0036] (4) 5g of citric acid is added to the complex solution described in step (3), stir evenly, adjust the pH to 5 with 1M NaOH solution, add water to 500ml, and vacuum filter with a 0.45 micron ultrafiltration membrane to obtain 2000ppm Colorless transparent nano-silver complex solution.
Embodiment 2
[0038] (1) 1g of nano-silver powder is added to 100ml of 2wt% PEG400 aqueous solution, and ultrasonically stirred for 1h to obtain a suspension of nano-silver;
[0039] (2) 5g ammonium persulfate is added to 850ml deionized water, stirred and dissolved to obtain ammonium persulfate solution;
[0040] (3) Add the ammonium persulfate solution described in step (2) into a 1L flask, heat in a water bath (50° C.), then add the nano-silver suspension solution described in step (1) to the ammonium persulfate solution, and continue the water bath Heating and stirring for 12 hours to obtain a complex solution;
[0041] (4) 5g tartaric acid is joined in the complex solution described in step (3), stir evenly, adjust pH to be 5 with 0.2M sodium carbonate solution, add water and be settled to 1000mL, vacuum filter with 0.45 micron ultrafiltration membrane, obtain 1000ppm colorless and transparent nano-silver complex solution.
Embodiment 3
[0043] (1) 20g of nano-silver powder was added to 1000mL of 5wt% PVP aqueous solution, and ultrasonically stirred for 3h to obtain a suspension of nano-silver;
[0044] (2) 50g potassium persulfate is added to 900ml deionized water, stirred and dissolved to obtain a strong oxidation complexing agent solution;
[0045] (3) The strong oxidation complexing agent solution described in step (2) is added in the 5L flask, and water bath heating (65 ℃), adds the nano-silver described in step (1) again in the super strong oxidation complexing agent solution Suspend the solution, continue heating and stirring in a water bath for 24 hours to obtain a complex solution;
[0046] (4) Add 10 g of citric acid to the complex solution described in step (3), stir evenly, adjust the pH to 7.5 with 0.2M sodium silicate solution, add water to 2000 mL, and vacuum filter with a 0.45 micron ultrafiltration membrane , to obtain 10000ppm colorless and transparent nano-silver complex solution.
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 