Integrally-formed hard fireproof strip
A fire-resistant strip and hard technology, applied in fire doors, building components, door/window applications, etc., can solve the problems of no expansion, complex process, fire performance impact, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0036] 1-1 Raw material composition of hard plastic shell
[0037] Including 30 parts by weight of polyvinyl chloride, 30 parts by weight of hydrogenated styrene-butadiene copolymer SEBS, 20 parts by weight of silica filler, 5 parts by weight of ammonium polyphosphate flame retardant and 5 parts by weight of tributyl phosphate plasticizer .
[0038] 1-2 Raw material composition of expandable graphite inner core
[0039]
[0040] 1-3 Preparation of fire strip
[0041] The expandable graphite inner core raw material and the hard plastic outer shell raw material are respectively put into corresponding parts of the extruder, the extrusion temperature is controlled at 140-160° C., extruded, embossed, and cooled to obtain the fireproof strip.
Embodiment 2
[0043] Other conditions are the same as in Example 1, except that in the raw material composition of 2-1 hard plastic casing, the consumption of polyvinyl chloride resin is 50 parts by weight, and the consumption of hydrogenated styrene-butadiene copolymer SEBS is 10 parts by weight share.
Embodiment 3
[0045] Other conditions are the same as in Example 2, except that in the raw material composition of 3-1 hard plastic casing, the amount of polyvinyl chloride resin is 60 parts by weight.