Hydrophobic breathable inorganic dry powder nanometer protective coating
An inorganic dry powder, hydrophobic and breathable technology, which is applied in coatings and other directions, can solve the problems of environmental protection characteristics of coatings, the influence of breathability and decorative effects, breathability of difficult-to-volatile harmful substances, space requirements for transportation and storage, and high cost. Achieve the effect of maintaining color and texture decoration, improving suspension stability, and simple and easy construction
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0060] Redispersible latex powder 14%
[0061] Ash Calcium 20%
[0062] Glass Powder 47%
[0063] Nano silica 6%
[0064] Light calcium carbonate 3%
[0065] Talc 8%
[0066] Bentonite 0.6%
[0067] Humectant 0.5%
[0068] Dispersant 0.3%
[0069] Water reducer 0.3%
[0070] Defoamer 0.3%
[0071] The sum of the weight percentages of the above-mentioned raw materials is 100%.
[0072] Weigh raw materials by weight, fully mix uniformly according to the aforementioned preparation method, obtain inorganic dry powder nano protective coating; mix according to the amount that the weight ratio of dry powder coating and water of the present invention is 1:3.5, obtain powder-water mixture after stirring uniformly, use Two methods of spraying and rolling are applied to the surface of the protective coating (textured dry powder coating sample) twice respectively to obtain a transparent thin protective coating film.
[0073] Use the lever micrometer method to measure the thickne...
Embodiment 2
[0075] Redispersible latex powder 20%
[0076] Ash Calcium 12%
[0077] Glass Powder 51%
[0078] Nano Silica 3%
[0079] Light calcium carbonate 2%
[0080] Talc 10%
[0081] Bentonite 0.6%
[0082] Humectant 0.5%
[0083] Dispersant 0.3%
[0084] Water reducer 0.3%
[0085] Defoamer 0.3%
[0086] The sum of the weight percentages of the above-mentioned raw materials is 100%.
[0087] Weigh raw materials by weight, fully mix uniformly according to the aforementioned preparation method, obtain inorganic dry powder nano protective coating; mix according to the amount that the weight ratio of dry powder coating and water of the present invention is 1:3.5, obtain powder-water mixture after stirring uniformly, use Spray evenly on the surface of the coating to be protected (textured dry powder coating sample) twice to obtain a transparent thin protective coating.
Embodiment 3
[0089] Redispersible latex powder 15%
[0090] Ash Calcium 17%
[0091] Glass Powder 53%
[0092] Nano Silica 3%
[0093] Light calcium carbonate 5%
[0094] Talc 5%
[0095] Bentonite 0.6%
[0096] Humectant 0.5%
[0097] Dispersant 0.3%
[0098] Water reducer 0.3%
[0099] Defoamer 0.3%
[0100] The sum of the weight percentages of the above-mentioned raw materials is 100%.
[0101] Weigh raw materials by weight, fully mix uniformly according to the aforementioned preparation method, obtain inorganic dry powder nano protective coating; mix according to the amount that the weight ratio of dry powder coating and water of the present invention is 1:3.5, obtain powder-water mixture after stirring uniformly, use Spray evenly on the surface of the coating to be protected (textured dry powder coating sample) twice to obtain a transparent thin protective coating.