Mixed-color core-spun yarn and production device and production method thereof
A production method and production device technology, applied in the field of textile yarns, can solve the problems of not being easy to wear next to the body, itching, poor releaseability, etc., and achieve the effects of obvious elasticity and functional characteristics, easy protection or sealing, and good shape retention
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Example Embodiment
[0043] Example 1
[0044] The preparation method of roving B in the present embodiment is as follows:
[0045] The raw material fibers of the roving B are 40% spun silk staple fibers and 60% cotton; 10wt% of the raw cotton fibers are blue;
[0046] Said preparation is obtained by a method comprising the following steps:
[0047] 1) The elastic short fibers of the elastic silk and the cotton fibers are mixed to form a mixed raw material;
[0048] 2) the mixed raw materials are made into cotton laps in the cleaning process, and the cotton lap is quantitatively 420 g / m; the cotton lap length is 36 meters;
[0049] 3) The cotton lap is combed into sliver on the carding machine; the raw sliver weight is 22 g / 5 m; the doffer speed is 20 rpm; ;
[0050] 4) The raw sliver is combined and drawn for three times on the drawing frame to form a sliver; the final sliver is quantitatively 20.5g / 5m; the number of slivers is 8;
[0051] 5) Draft the sliver into roving B on the roving frame;...
Example Embodiment
[0065] Example 2
[0066] This embodiment is a blended core-spun yarn for fine-count wool-containing knitted sweaters.
[0067] Roving B is prepared by a method comprising the following steps:
[0068] 1) The raw material fibers of the roving B are: 60wt% wool, 40wt% cotton; cotton fibers have 10wt% black;
[0069] 2) The wool fiber can also be pre-treated to prevent its electrostatic effect;
[0070] 3) Mix wool fiber and cotton fiber to form mixed fiber;
[0071] 4) The mixed fibers are made into laps in the cleaning process, and the ration of the laps is 420 g / m; the length of the laps is 36 meters;
[0072] 5) Comb the laps on the carding machine to form sliver; the sliver weight is 18-24 g / 5 m; the doffer speed is 15-22 rpm; the distance between the cover plate and the cylinder clothing is 8, 7, 6 ,6,7;
[0073] 6) The raw sliver is combined and drafted for three times on the drawing frame to form a sliver; the sliver is quantitatively 20.5g / 5m at the end; the number...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap