Bone-imitation composite material scaffold and preparation method thereof

A composite material and bone-like technology, which is applied in medical science, tissue regeneration, prosthesis, etc., can solve the problems of incomplete degradation, large difference in bone modulus, and weak osteogenic performance, so as to achieve easy production, popularization and application, The effect of good biocompatibility and broad application prospects

Active Publication Date: 2020-06-09
SICHUAN UNIV
View PDF11 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] Specifically, natural polymer materials such as collagen, fibrin, and chitosan have good biocompatibility and can provide a natural three-dimensional porous structure for cell adhesion, proliferation, and differentiation, but they have poor mechanical properties, which are comparable to human bone modulus. The difference is large, and further modification and enhancement are needed
Synthetic polymers such as polyglycolic acid (PGA), polylactic acid (PLA) and polycaprolactone (PCL) are easy to process and have excellent biocompatibility and degradability, but there are also some disadvantages: hydrophilicity Poor, insufficient mechanical strength, degraded products have certain influence
However, calcium-phosphorus ceramics and bioactive glass have high mechanical strength and good biocompatibility, but they are easy to break or cannot be completely degraded, and have their own shortcomings.
Due to the problems of poor mechanical strength or weak osteogenic performance of a single material, it is difficult to meet the high requirements of bone tissue engineering scaffold materials by using the above materials alone

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Bone-imitation composite material scaffold and preparation method thereof
  • Bone-imitation composite material scaffold and preparation method thereof
  • Bone-imitation composite material scaffold and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0037] (1) Preparation of natural cellulose scaffold material

[0038] Measure 100 mL of acetic acid-sodium acetate buffer solution, weigh 3.5 g of sodium chlorite into the buffer solution, stir evenly to dissolve it, and prepare a lignin removal solution. Immerse the beech wood chips in the lignin removal solution, and stir slowly at 60°C for 36 hours, then take out the wood chips, rinse with deionized water for 5 minutes, soak and ultrasonicate for 5 minutes, repeat three times, and then soak in deionized water for 24 hours. The wood chip samples were taken out, rinsed with deionized water, and freeze-dried for 12 hours.

[0039] (2) Fabrication of HA cellulose scaffolds

[0040] Prepare 0.5mol / L calcium nitrate solution, adjust the pH to 11 with ammonia water, put the natural cellulose stent into 50mL calcium nitrate solution, soak for 8 hours, take out the stent sample; then prepare 0.5mol / L diammonium hydrogen phosphate solution , adjust the pH to 11 with ammonia water,...

Embodiment 2

[0045] (1) Preparation of natural cellulose scaffold material

[0046]Measure 100 mL of acetic acid-sodium acetate buffer solution, weigh 10 g of sodium chlorite into the buffer solution, stir evenly to dissolve it, and prepare a lignin removal solution. Immerse the pine wood chips in the lignin removal solution, and stir slowly under the condition of 70°C for 24 hours, then take out the wood chips, rinse with deionized water for 10 minutes, soak and ultrasonicate for 10 minutes, repeat three times, and then soak in deionized water for 24 hours. The wood chip samples were taken out, rinsed with deionized water, and freeze-dried for 18 hours.

[0047] (2) Fabrication of HA cellulose scaffolds

[0048] Prepare 0.2mol / L calcium nitrate solution, adjust the pH to 11 with ammonia water, put the natural cellulose stent into 60mL calcium nitrate solution, soak and react for 12h, take out the stent sample; then prepare 0.2mol / L diammonium hydrogen phosphate solution , adjust the pH ...

Embodiment 3

[0053] (1) Preparation of natural cellulose scaffold material

[0054] Measure 100 mL of acetic acid-sodium acetate buffer solution, weigh 10 g of sodium chlorite into the buffer solution, stir evenly to dissolve it, and prepare a lignin removal solution. Immerse the beech wood chips in the lignin removal solution, and stir slowly at 70°C for 24 hours, then take out the wood chips, rinse with deionized water for 10 minutes, soak and ultrasonicate for 10 minutes, repeat three times, and then soak in deionized water for 24 hours. The wood chip samples were taken out, rinsed with deionized water, and freeze-dried for 18 hours.

[0055] (2) Preparation of PCL composite HA cellulose bone-like composite scaffold

[0056] Dissolve 5g of polycaprolactone and 5g of nano-hydroxyapatite in 40g of 1,4-dioxane solution, and stir vigorously at 40°C until the polycaprolactone is completely dissolved and the nano-hydroxyapatite is fully dispersion. Place the natural cellulose stent prepare...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention provides a bone-imitation composite material scaffold and a preparation method thereof. The method comprises the following steps: performing delignification treatment on natural wood, performing compounding by using hydroxyapatite to obtain a bone-inducible scaffold material, and performing infiltration by using polycaprolactone to simulate an extracellular matrix to obtain the bone-imitation composite material scaffold. The method obtains the highly anisotropic porous scaffold, the three-dimensional pore structure provides channels for nutrient substance transportation and intracellular growth and regeneration, the shortcomings of traditional isotropic scaffold materials are overcome, and the strength and stability requirements of bone tissue regeneration are met; and the method does not need to use special reagents or equipment, is not difficult to operate and mild in process conditions, and has the characteristics of easy realization of production, promotion and application.

Description

technical field [0001] The invention belongs to the field of composite materials, and in particular relates to a bone-like composite material bracket and a preparation method thereof. Background technique [0002] Bio-scaffold materials are directly applied inside the human body and facing the complex and sensitive system of the human body, people have various and extremely high requirements for bio-scaffold materials. Therefore, the bioscaffold material must have the following characteristics: (1) good biocompatibility, it cannot have immunogenicity or cytotoxicity and cause unresolved inflammatory reactions; (2) certain mechanical strength and mechanical properties, in the operation It will not collapse during operation and normal patient activities; (3) easy to sterilize to prevent bacterial infection; (4) facilitate cell adhesion and proliferation; (5) controllable interconnected pores to guide cells to grow into the desired physical Forms and promotes vascularization o...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): A61L27/12A61L27/18A61L27/20A61L27/50A61L27/56A61L27/58
CPCA61L27/12A61L27/18A61L27/20A61L27/50A61L27/56A61L27/58A61L2430/02C08L97/02C08L67/04
Inventor 楚合涛刘晋明李建树
Owner SICHUAN UNIV
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products