Scheelite flotation collecting agent
A collector and scheelite technology, which is applied in the field of mineral flotation collectors and flotation collectors, can solve the problems of production index decline, high flotation temperature requirements, and large dosage of chemicals, so as to achieve easy operation and control , improved flotation, simple preparation method
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0026] The scheelite flotation collector of this embodiment is prepared from the following raw materials in weight percentage: 32% tetrasodium sulfosuccinic acid, 65% sodium fatty acid, 1% water glass, and 2% sodium fluoride , weigh the raw materials respectively according to the above weight percentage, heat fatty acid sodium to 60°C-70°C, add tetrasodium sulfosuccinic acid and stir, then add water glass and sodium fluoride and stir for 1.5 hours, stir well, Prepare scheelite flotation collector.
[0027] Using the prepared scheelite flotation collector, the flotation grade of the raw ore is 0.43%, and the obtained titanium concentrate grade reaches 1.21%, and the recovery rate is a good indicator of 89.11%.
Embodiment 2
[0029] The scheelite flotation collector of this embodiment is prepared from the following raw materials in weight percentage: 34% tetrasodium sulfosuccinic acid, 63% sodium fatty acid, 1% water glass, and 2% sodium fluoride , weigh the raw materials respectively according to the above weight percentage, heat fatty acid sodium to 60°C-70°C, add tetrasodium sulfosuccinic acid and stir, then add water glass and sodium fluoride and stir for 1.5 hours, stir well, Prepare scheelite flotation collector.
[0030] Using the prepared scheelite flotation collector, the flotation grade of the raw ore is 0.43%, and the obtained titanium concentrate grade reaches 1.21%, and the recovery rate is a good indicator of 89.45%.
Embodiment 3
[0032] The scheelite flotation collector of this embodiment is prepared from the following raw materials in weight percentage: 36% tetrasodium sulfosuccinic acid, 61% sodium fatty acid, 1% water glass, and 2% sodium fluoride , weigh the raw materials respectively according to the above weight percentage, heat fatty acid sodium to 60°C-70°C, add tetrasodium sulfosuccinic acid and stir, then add water glass and sodium fluoride and stir for 1.5 hours, stir well, Prepare scheelite flotation collector.
[0033] Using the prepared scheelite flotation collector, the flotation grade of the raw ore is 0.43%, and the obtained titanium concentrate grade reaches 1.24%, and the recovery rate is a good indicator of 89.51%.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com