A method for recovering fine-grained pyrite from sulfur-containing slime tailings
A technology of sulfur-containing ore and pyrite, which is applied in the direction of solid separation and flotation, can solve the problems of environmentally harmful secondary ore slime tailings, loss of fine-grained pyrite, and reduction of metal recovery rate, etc., to achieve selectivity Ideal effect, increase floating difference, and easy operation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0047] like figure 2 As shown, the sulfur-containing slime tailings of this embodiment contain 7.42 wt % of sulfur, and the fineness is -0.019 mm, and the minerals account for 80 wt %. Among them, the main metal minerals are pyrite, with a small amount of chalcopyrite, and the gangue minerals are mainly quartz, feldspar, mica, kaolinite and montmorillonite.
[0048] (1) Concentration and dehydration: the sulfur-containing mud tailings slurry with sulfur content of 7.42wt%, concentration of 10wt%, and fineness of -0.019mm granular minerals accounting for 80wt% was first concentrated to a slurry concentration of 22wt% by a thickener, Then, it is concentrated under the condition of rotating speed of 2770r / min by a horizontal screw centrifuge, so that the mass concentration of the pulp reaches 50wt%, and the water and the residual flotation agent in the pulp are removed;
[0049] (2) Slurry mixing: add water to the concentrated ore pulp to adjust the slurry to a concentration of...
Embodiment 2
[0055] The sulfur-containing slime tailings of this embodiment contain 5.89 wt % of sulfur, and the minerals with a fineness of -0.019 mm account for 82 wt %. Among them, the main metal minerals are pyrite, with a small amount of chalcopyrite, and the gangue minerals are mainly quartz, feldspar, mica, kaolinite and montmorillonite.
[0056] (1) Concentration and dehydration: the sulfur-containing slime tailings slurry with sulfur content of 5.89wt%, concentration of 8wt%, and fineness of -0.019mm granular minerals accounting for 90wt% is first concentrated to a slurry concentration of 18wt% by a thickener, Then, it is concentrated under the condition of rotating speed of 2920r / min through a horizontal screw centrifuge, the mass concentration of the pulp reaches 55wt%, and the water and the residual flotation agent in the pulp are removed;
[0057] (2) Slurry mixing: add water to the concentrated ore pulp to adjust the slurry to a concentration of 25wt%, and add 300g / t of conce...
Embodiment 3
[0063] The sulfur-containing slime tailings in this embodiment contain 8.51 wt% of sulfur, and the fineness of -0.019mm size minerals accounts for 83 wt%. Among them, the main metal minerals are pyrite, with a small amount of chalcopyrite, and the gangue minerals are mainly quartz, feldspar, mica, kaolinite and montmorillonite.
[0064] (1) Concentration and dehydration: The sulfur-containing sludge tailings slurry with sulfur content of 8.51wt%, concentration of 12wt%, and fineness of -0.019mm granular minerals accounting for 83wt% was first concentrated to a slurry concentration of 25wt% by a thickener, and then Concentrate by horizontal screw centrifuge under the condition of rotating speed 2870r / min, the mass concentration of pulp reaches 52wt%, remove water and residual flotation agent in pulp;
[0065] (2) Slurry mixing: add water to the concentrated ore pulp to adjust the slurry to a concentration of 35wt%, and add 500g / t of concentrated sulfuric acid to the mixing barr...