Embodiment 1
[0034] Embodiment one: the application of urea-formaldehyde glue production blockboard
[0035] a. Take 300 grams of chemically pure propylene glycol, add 20 grams of chemically pure menthol, add 30 grams of chemically pure camphor and stir until completely dissolved, then add 50 grams of nano silver and mix evenly for later use;
[0036] B, get 50 kilograms of E0 urea-formaldehyde glue (free formaldehyde content 0.02%), add the additive prepared in step a under stirring, fully stir for 5 minutes and mix evenly, then add flour to adjust glue;
[0037] c. After the glue adjustment is completed, follow the normal process requirements of urea-formaldehyde glue to complete all steps such as glue coating, billet formation, cold pressing, and hot pressing to complete the entire production process (glue consumption: 2.8 kg / sheet). Samples were taken to test its free formaldehyde release, water content, dipping and peeling performance indicators, and anti-mildew effect in a normal tem...
Embodiment 2
[0040]Embodiment two: the application of melamine modified urea-formaldehyde glue to produce eucalyptus wood 11-layer multi-layer board
[0041] a. Take 200 grams of chemically pure propylene glycol, add 10 grams of chemically pure menthol, add 20 grams of chemically pure camphor and stir until completely dissolved, then add 10 grams of nano silver and mix evenly for later use;
[0042] b. Take 60 kg of melamine-modified urea-formaldehyde glue and add 240 grams of the solution prepared in step a under stirring, fully stir and mix evenly, and then add flour to adjust the glue;
[0043] c. After the glue adjustment is completed, follow the normal process requirements of urea-formaldehyde glue to complete all steps such as glue application, billet formation, cold pressing, and hot pressing, and complete the entire production process (the amount of glue used on one side is 180 grams per square meter). Samples were taken to test its free formaldehyde release, water content, bonding...
Embodiment 3
[0046] Example Three: Production and Application of Soybean Glue All Eucalyptus Floor Substrate
[0047] a. Take 300 grams of chemically pure propylene glycol, add 15 grams of chemically pure menthol, add 30 grams of chemically pure camphor and stir until completely dissolved, then add 30 grams of nano silver and mix evenly for later use;
[0048] b. Get 60 kilograms of soybean gum and add 375 grams of the mixed solution prepared in step a under stirring, fully stir and mix evenly, and then add 28 kilograms of defatted soybean powder to adjust the glue;
[0049] c. After the glue adjustment is completed, complete all steps such as glue coating, billet formation, cold pressing, and hot pressing according to the normal process requirements of urea-formaldehyde glue, and complete the entire production process (the amount of glue used on one side is 200 grams per square meter). Samples were taken to test its free formaldehyde release, water content, bonding strength, dipping and p...