Ilmenite flotation collecting agent
A collector and ilmenite technology, applied in the field of mineral flotation collectors and flotation collectors, can solve the problems of low selectivity, poor antifreeze ability, poor dispersibility, etc., and achieve the preparation method Simple, low-cost, stable effect of concentrate amount
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] The ilmenite flotation collector of this embodiment is prepared from the following raw materials by weight percentage: the weight percentage of Yiji Peng T is 13%. The weight percentage of sodium oleate is 72%. The weight percent of pinitol oil is 6%. The weight percentage of kerosene is 7%, and the weight percentage of the added amount of water glass is 2%.
[0028] Weigh the raw materials respectively according to the above weight percentage, heat sodium oleate to 60°C-70°C, add Iquipon T and stir, then add terpineol oil and kerosene and stir, finally add water glass and stir for 1 hour, stir Evenly, the ilmenite flotation collector is prepared.
[0029] Using the prepared ilmenite flotation collector, the flotation grade of raw ore is 20.11%, and the obtained titanium concentrate grade reaches 48.09%, and the recovery rate is a good indicator of 80.99%.
Embodiment 2
[0031] The ilmenite flotation collector of this embodiment is prepared from the following raw materials by weight percentage: the weight percentage of Yiji Peng T is 14%. The weight percent of sodium oleate is 70%. The weight percent of pinitol oil is 7%. The weight percentage of kerosene is 7%, and the weight percentage of the added amount of water glass is 2%.
[0032] Weigh the raw materials respectively according to the above weight percentage, heat sodium oleate to 60°C-70°C, add Iquipon T and stir, then add terpineol oil and kerosene and stir, finally add water glass and stir for 1 hour, stir Evenly, the ilmenite flotation collector is prepared.
[0033] Using the prepared ilmenite flotation collector, the flotation grade of raw ore is 20.11%, and the obtained titanium concentrate grade reaches 48.55%, and the recovery rate is a good indicator of 81.03%.
Embodiment 3
[0035] The ilmenite flotation collector of this embodiment is prepared from the following raw materials by weight percentage: the weight percentage of Yiji Peng T is 15%. The weight percentage of sodium oleate is 68%. The weight percent of pinitol oil is 8%. The weight percentage of kerosene is 7%, and the weight percentage of the added amount of water glass is 2%.
[0036] Weigh the raw materials respectively according to the above weight percentage, heat sodium oleate to 60°C-70°C, add Iquipon T and stir, then add terpineol oil and kerosene and stir, finally add water glass and stir for 1 hour, stir Evenly, the ilmenite flotation collector is prepared.
[0037] Using the prepared ilmenite flotation collector, the flotation grade is 20.11% of the raw ore, the obtained titanium concentrate grade is 48.36%, and the recovery rate is a good indicator of 80.26%.