Carbon dioxide electrolysis device and carbon dioxide electrolysis method
A carbon dioxide and electrolysis technology, applied in the electrolysis process, electrolysis components, cells, etc., can solve the problems of toxic gases and complex chemical products, and achieve the effects of efficient storage, simplified gas management, and rational utilization.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] First, in step S1, the Li 2 CO 3 、Na 2 CO 3 After the two carbonates were mixed in a molar ratio of 2:1, they were placed in an airtight container and dried at 150°C for 12 hours.
[0033] Next, in step S2, the electrolyte material prepared in step S1 is put into the electrolytic container for pre-electrolysis. At this time, the first electrolysis voltage was set to 0.8V, the first electrolysis time was 1 hour, and the first electrolysis temperature was 300°C. During pre-electrolysis, a constant and steady supply of carbon dioxide to the electrolysis vessel is always maintained.
[0034] Then, in step S3, enter the formal electrolysis. At this time, the second electrolysis voltage was set to 2V, the second electrolysis temperature was 300° C., and the carbon dioxide was continuously and stably supplied to the electrolysis container.
Embodiment 2
[0036] First, in step S1, the Li 2 CO 3 、K 2 CO 3 After the two carbonates were mixed in a molar ratio of 3:1, they were placed in an airtight container and dried at 250°C for 48 hours.
[0037] Next, in step S2, the electrolyte material prepared in step S1 is put into the electrolytic container for pre-electrolysis. At this time, the first electrolysis voltage was set to 2V, the first electrolysis time was 2 hours, and the first electrolysis temperature was 300°C. During pre-electrolysis, a constant and steady supply of carbon dioxide to the electrolysis vessel is always maintained.
[0038] Then, in step S3, enter the formal electrolysis. At this time, the second electrolysis voltage was set to 6V, and the second electrolysis temperature was set to 700° C., so that carbon dioxide was continuously and stably supplied to the electrolysis container.
Embodiment 3
[0040] First, in step S1, the Li 2 CO3, Na 2 CO 3 、K 2 After mixing the three CO3 carbonates according to the molar ratio of 4:3:3, they were placed in an airtight container and dried at 200°C for 48 hours.
[0041] Next, in step S2, the electrolyte material prepared in step S1 is put into the electrolytic container for pre-electrolysis. At this time, the first electrolysis voltage was set to 1.6V, the first electrolysis time was 2 hours, and the first electrolysis temperature was 500°C. During pre-electrolysis, a constant and steady supply of carbon dioxide to the electrolysis vessel is always maintained.
[0042] Then, in step S3, enter the formal electrolysis. At this time, the second electrolysis voltage is set to 4V, the second electrolysis temperature is 450° C., and the carbon dioxide is continuously and stably supplied to the electrolysis container.