Novel rubber concrete material and preparation method thereof
A rubber concrete, a new type of technology, applied in the field of rubber materials, can solve the problems of difficulty in controlling the degree of delamination, weak adhesion between rubber particles and cement, and uneven distribution of rubber, so as to ensure uniformity, increase water retention, and improve The effect of early strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0031] A novel rubber concrete material comprising components by weight of:
[0032]
[0033] A kind of preparation method of novel rubber concrete, comprises the following steps:
[0034] Step 1, obtain the following components by weight:
[0035]
[0036]
[0037] Step 2, mixing rubber particles, sand, and cement evenly to obtain a rubber-sand-cement mixture;
[0038] Step 3, mixing water, water reducing agent, and hydroxypropyl methylcellulose and stirring evenly to obtain a mixed solution;
[0039] Step 4, pouring the mixed solution in step 3 into the rubber-sand-cement mixture in step 2 in 2 to 3 times, pouring the mixed solution while stirring, and finally obtaining a slurry;
[0040] Step 5: pour the slurry obtained in step 4 within 15 minutes until the mold is vibrated, and after standing for 2 to 3 hours, the mold can be removed for maintenance to obtain rubber concrete.
[0041] Preferably, the particle size of the rubber particles is 0.075-0.25 mm.
[0...
Embodiment 2
[0048] A kind of preparation method of novel rubber concrete, comprises the following steps:
[0049] Step 1, obtain the following components by weight:
[0050]
[0051] Step 2, mixing 225g of rubber particles, 225g of sand, and 300g of sulfoaluminate cement to obtain a rubber-sand-cement mixture;
[0052] Step 3, mix 250g of water, 2.5g of water reducer, and 0.75g of hydroxypropyl methylcellulose and stir evenly to obtain a mixed solution;
[0053] Step 4, pour the mixed solution in step 3 into the rubber-sand-cement mixture in step 2 in 3 times, pour the mixed solution while stirring, and finally obtain the slurry;
[0054] Step 5: pour the slurry obtained in step 4 within 15 minutes until the mold is vibrated, and after standing for 2 to 3 hours, the mold can be removed for maintenance to obtain rubber concrete.
[0055] In this embodiment, the particle size of rubber particles is 0.075-0.25 mm; the particle size of sand is 0.5-1 mm; the cement is sulfoaluminate cemen...
PUM
| Property | Measurement | Unit |
|---|---|---|
| particle diameter | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 