Foamed asphalt mixture and preparation method thereof

A foamed asphalt and mixture technology, which is applied in the field of foamed asphalt mixture and its preparation, can solve the problems of long heating time of asphalt and easy production of harmful substances, etc., and achieve the improvement of plastic deformation resistance, energy saving and environmental protection production and construction requirements, and improve work efficiency Effect

Active Publication Date: 2022-05-13
广东广基建设集团有限公司
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0004] At present, when preparing foamed asphalt mixture, it is first necessary to heat the asphalt, and then inject foaming water into the heated asphalt, and the asphalt mixture will expand instantaneously through water evaporation and then return to its original state. However, the above preparation process often requires Only by heating the asphalt to a higher temperature can it be stably combined with the foaming water, so the heating time of the asphalt is long, and harmful substances are likely to be produced during the heating process, which is a factor that restricts the more effective promotion of foamed asphalt mixture

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Foamed asphalt mixture and preparation method thereof
  • Foamed asphalt mixture and preparation method thereof
  • Foamed asphalt mixture and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0049] A kind of foam asphalt mixture is prepared by the following steps:

[0050]Step 1: After mixing 10.5kg of SBS modified asphalt, 0.25kg of first component water and 85kg of old asphalt pavement milling material for 20s, add 2.4kg of cupro ammonia fiber, 1.5kg of antimony trioxide and 0.7kg of 2,2'-di Hydroxy-4,4'-dimethoxybenzophenone is then heated to 70°C and stirred for 40s to obtain primary foam asphalt mixture;

[0051] Step 2, mixing the primary foamed asphalt mixture with 0.25kg of the second component water for 35s, after secondary foaming, crushing and screening into A material with a particle size of 0-9.5mm and B material with a particle size of 9.5-19mm;

[0052] Step 3: Stir and mix 60kg of material A, 40kg of material B, 35kg of gravel and 1.2kg of cement in proportion for 40 seconds to obtain foamed asphalt mixture.

Embodiment 2

[0054] A kind of foam asphalt mixture is prepared by the following steps:

[0055] Step 1: After mixing 10.5kg of SBS modified asphalt, 0.25kg of first component water and 85kg of old asphalt pavement milling material for 30s, add 2.4kg of cupro ammonia fiber, 1.5kg of antimony trioxide and 0.7kg of 2,2'- After dihydroxy-4,4'-dimethoxybenzophenone, the temperature was raised to 90°C and stirred for 30s to obtain the primary foamed asphalt mixture;

[0056] Step 2, mixing the primary foamed asphalt mixture with 0.25kg of the second component water for 25s, after secondary foaming, crushing and screening into material A with a particle size of 0-9.5mm and material B with a particle size of 9.5-19mm;

[0057] Step 3: Stir and mix 60kg of material A, 40kg of material B, 35kg of gravel and 1.2kg of cement in proportion for 55s to obtain foamed asphalt mixture.

Embodiment 3

[0059] A kind of foam asphalt mixture is prepared by the following steps:

[0060] Step 1: After mixing 10.5kg of SBS modified asphalt, 0.25kg of first component water and 85kg of old asphalt pavement milling material for 25s, add 2.4kg of cupro ammonia fiber, 1.5kg of antimony trioxide and 0.7kg of 2,2'- After dihydroxy-4,4'-dimethoxybenzophenone, the temperature was raised to 81°C and stirred for 34s to obtain the primary foamed asphalt mixture;

[0061] Step 2, mixing the primary foamed asphalt mixture with 0.25kg of the second component water for 32s, after secondary foaming, crushing and screening into A material with a particle size of 0-9.5mm and B material with a particle size of 9.5-19mm;

[0062] Step 3: Stir and mix 60kg of material A, 40kg of material B, 35kg of gravel and 1.2kg of cement in proportion for 52s to obtain a foamed asphalt mixture.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
particle diameteraaaaaaaaaa
Login to view more

Abstract

The invention relates to the field of asphalt mixed building materials, in particular to a foamed asphalt mixture and a preparation method thereof. The foamed asphalt mixture is prepared from the following raw materials in parts by weight: matrix asphalt; water; regenerating cellulose fibers; collecting materials; cement; antimony trioxide; the solvent is 2, 2 '-dihydroxy-4, 4'-dimethoxy benzophenone; the preparation method comprises the following steps: mixing the matrix asphalt, the water and the old asphalt pavement milling material, adding the regenerated cellulose fibers, the antimony trioxide and the 2, 2 '-dihydroxy-4, 4'-dimethoxybenzophenone, heating and mixing to obtain a primary foamed asphalt mixture; mixing the primary foamed asphalt mixture with water, carrying out secondary foaming, and then crushing and screening to obtain a material A and a material B; the material A, the material B, the aggregate and the cement are stirred and mixed in proportion, the foamed asphalt mixture is obtained, and the foamed asphalt mixture has the effects that the temperature for stable combination of foaming water and hot asphalt can be reduced, and meanwhile the construction efficiency is improved.

Description

technical field [0001] The application relates to the field of asphalt mixed building materials, more specifically, it relates to a foamed asphalt mixture and a preparation method thereof. Background technique [0002] Asphalt mixture is a general term for mixtures made by mixing mineral aggregates and asphalt binders. It is a composite material mainly composed of asphalt, coarse aggregate, fine aggregate, and mineral powder. [0003] Nowadays, in the building pavement construction industry, in order to meet the requirements of energy saving and environmental protection, people generally use recycled materials to prepare asphalt mixture, and then pave the road surface. However, the existing foamed asphalt mixture has fast rolling forming and stable performance. Therefore, it is widely used in the laying of asphalt pavement. [0004] At present, when preparing foamed asphalt mixture, it is first necessary to heat the asphalt, and then inject foaming water into the heated asp...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C04B26/26C04B38/02C04B16/06C04B14/30C04B24/02
CPCC04B26/26C04B38/02C04B16/06C04B14/30C04B24/023C04B2111/0075C04B18/16C04B14/02C04B14/00C04B22/002Y02W30/91
Inventor 林达宇林丹玫庞金玲林达周蒙新黄永斌叶少杰罗增练廖家竟林达权黄正添陈华昌
Owner 广东广基建设集团有限公司
Who we serve
  • R&D Engineer