Embodiment 1
[0023] In terms of weight percentage, prepare 19.55 parts of water, 21 parts of titanium dioxide, 34 parts of emulsion, 2 parts of wax emulsion, 0.15 part of fungicide, 0.25 part of HEC thickener (hydroxyethyl cellulose), 0.1 part of organic amine (AMP95) , 0.6 parts of aliphatic defoamer, 0.35 parts of acrylate ammonium salt dispersant, 0.3 parts of non-ionic silicone copolymer wetting agent, 2 parts of propylene glycol, 5 parts of kaolin, 4 parts of talc, 8 parts of calcium carbonate, 0.4 parts of carbendazim, 1.3 parts of alcohol ester twelve, 1 part of PU thickener, made as follows:
[0024] 1) First add 18.5 parts of water, bactericide, HEC thickener, organic amine, 0.3 parts of defoamer, dispersant, wetting agent, and propylene glycol into the mixer, and disperse at high speed for 5 minutes at a speed of 1200 rpm;
[0025] 2) Then add titanium dioxide, kaolin, talcum powder, and calcium carbonate, and continue to disperse at high speed for 30 minutes at a speed of 1200 r...
Embodiment 2
[0029] In terms of weight percentage, prepare 21 parts of water, 18 parts of titanium dioxide, 32 parts of emulsion, 1.5 parts of wax emulsion, 0.1 part of fungicide, 0.2 part of HEC thickener (hydroxyethyl cellulose), 0.2 part of organic amine (AMP95) 0.4 parts of aliphatic defoamer, 0.3 parts of acrylate ammonium salt dispersant, 0.2 parts of non-ionic siloxane copolymer wetting agent, 2.5 parts of propylene glycol, 7 parts of kaolin, 5 parts of talc, 9 parts of calcium carbonate , 0.3 part of n-octylisothiazolinone, 1.5 part of alcohol ester twelve, 0.8 part of PU thickener, make as follows:
[0030] 1) First add 20 parts of water, bactericide, HEC thickener, organic amine, 0.2 parts of defoamer, dispersant, wetting agent, and propylene glycol into the mixer, and disperse at high speed for 5 minutes at a speed of 1200 rpm;
[0031] 2) Then add titanium dioxide, kaolin, talcum powder, and calcium carbonate, and continue to disperse at high speed for 35 minutes at a speed of ...
Embodiment 3
[0035] In terms of weight percentage, prepare 17 parts of water, 22.6 parts of titanium dioxide, 31 parts of emulsion, 3 parts of wax emulsion, 0.2 part of fungicide, 0.35 part of HEC thickener (hydroxyethyl cellulose), organic amine (AMP95) 0.15 parts, 0.15 parts of aliphatic defoamer, 0.15 parts of acrylate ammonium salt dispersant, 0.15 parts of non-ionic silicone copolymer wetting agent, 3.5 parts of propylene glycol, 3 parts of kaolin, 6 parts of talc, 10 parts of calcium carbonate Part, 0.25 part of n-octylisothiazolinone, 1.6 part of alcohol ester twelve, 0.75 part of PU thickener, make as follows:
[0036] 1) First add 16.5 parts of water, bactericide, HEC thickener, organic amine, 0.15 parts of defoamer, dispersant, wetting agent, and propylene glycol into the mixer, and disperse at high speed for 5 minutes at a speed of 1200 rpm;
[0037] 2) Then add titanium dioxide, kaolin, talcum powder, and calcium carbonate, and continue to disperse at high speed for 35 minutes ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com