Process for preparing poly modified chitosan anti-bacteria wet keeping finishing agent
A technology of chitosan and finishing agent, applied in fiber processing, textiles and papermaking, etc., can solve the problems of no antibacterial properties, aldehyde pollution, no moisture retention, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
example 1
[0016] Formula: chitosan, dosage 5%; sodium pyrrolidone carboxylate, dosage 7%; silver acetate (CH 3 COOAg), the dosage is 2.4%; softener, 5%; water, the balance; all are by weight.
[0017] Preparation process: firstly, chitosan is prepared into 8% acid solution, and the cosolvent is inorganic acid or organic acid. Silver acetate (CH 3 COOAg), react for 30 to 60 minutes, then add sodium pyrrolidone carboxylate and react for 60 minutes to obtain a finishing agent mother liquor; finally, add 25% nonionic softener (fatty acid polyoxyethylene ether), continue stirring for 15 minutes, and add water to dilute The antibacterial moisturizing finishing agent for textiles is obtained when the formula content is reached.
[0018] Application process: test fabric, polyester-cotton plain weave; the dosage of antibacterial moisturizing finishing agent is 10% (owf).
[0019] Technological process: polyester-cotton plain weave → two dipping and two rolling (with liquid rate 100%) → hot ai...
example 2
[0021] Formula: chitosan, dosage 3.6%; ammonium pyrrolidone carboxylate, dosage 10.5%; silver nitrate (AgNO 3 ), dosage 2.8%; sodium alginate 7.2%; water, balance.
[0022] Preparation process: firstly, chitosan is prepared into a 7% acid solution, and the cosolvent is an inorganic acid or an organic acid. Silver nitrate (AgNO 3 ), reacted for 50 minutes, then added ammonium pyrrolidone carboxylate and reacted for 70 minutes, and finally added sodium alginate and reacted for 30 to 60 minutes to obtain the finishing agent mother liquor. Finally, adding or not adding softening agent and adhesive as required, and adding water to dilute to formula content to obtain antibacterial moisturizing finishing agent for textiles.
[0023] Application process: test fabric, pure cotton poplin; the dosage of antibacterial moisturizing finishing agent is 10% (owf).
[0024] Technological process: pure cotton poplin cloth → two dipping and two rolling (with liquid rate 100%) → hot air drying...
example 3
[0026] Formula: chitosan, dosage 3.6%; sodium pyrrolidone carboxylate, dosage 10.5%; nitrate (AgNO 3 ) dosage 2.8%; sodium alginate 7.2%; water, balance; all are weight ratios.
[0027] Preparation process: firstly, chitosan is prepared into a 2% acid solution, and the cosolvent is an inorganic acid or an organic acid. Nitrate (AgNO 3 ), react for 70 minutes, then add sodium pyrrolidone carboxylate to react for 55 minutes, and finally add sodium alginate to react for 40 to 60 minutes to obtain finishing agent mother liquor. Finally, softener and adhesive are added or not added as required, and water is added to dilute to formula content to obtain antibacterial moisturizing finishing agent for textiles.
[0028] Application process: test fabric, linen fabric; the dosage of antibacterial moisturizing finishing agent is 5% (owf).
[0029] Technological process: linen fabric → two dips and two rollings (with liquid rate of 100%) → hot air drying (temperature 90 ° C ~ 100 ° C) →...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com