A stone paper and coating technology, applied in paper coating, special paper, papermaking, etc., can solve the problems of difficult recycling and secondary environmental pollution application, and achieve the effects of easy deinking, easier control of process parameters, and reduced environmental pollution
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0034] According to the formula, 30% acrylic resin (such as J678 resin of Taiwan Johnson Company), 47.7% deionized water, 2% ammonia water, and then take 20% waste ceramic powder, stir, disperse and put it into a 2L sander for grinding; 3 hours Finally, take it out and put it into a stirred container, finally add 0.2% antistatic agent and 0.1% defoamer (such as 0506 defoamer from Taiwan Deqian Company), and stir for 30 minutes to make stone paper coating. The scraping test on PET stone paper film has good effect and meets the requirements. According to GB / T13217 "Gravure Plastic Ink Test Method" and GB / T 6753.3 "Paint Storage Stability Test Method", the test results are fineness ≤ 15 microns; viscosity 80 seconds (4 cups, 25 ℃); initial dryness 30 mm .30 seconds, adhesion fastness 90%, good stability.
Embodiment 2
[0036] 40% acrylic resin (such as the J678 resin of Taiwan SC Johnson Company), 46.2% deionized water, 3% ammonia water, get 10% waste ceramic powder again, stir, put into 2L grinder after dispersing and grind; Take out after 3 hours and Put it into a stirred container, finally add 0.5% antistatic agent and 0.3% defoamer (such as 0506 defoamer from Taiwan Deqian Company), and stir for 30 minutes to make stone paper coating. The scraping test on PET stone paper film has good effect and meets the requirements. According to GB / T 13217 "Gravure Plastic Ink Test Method" and GB / T 6753.3 "Paint Storage Stability Test Method", the test results are fineness ≤ 10 microns; viscosity 70 seconds (4 cups, 25 ℃); initial dryness 30 mm.30 seconds, adhesion fastness 90%, good stability.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com