Aqueous environmentally-friendly leather finishing and delustering handfeel wax assistant and preparation process thereof
A wax additive and an environmentally friendly technology, which is applied in the field of water-based environmental protection leather coating matting handle wax additives, can solve the problems of strong optical reflection, environmental pollution, and difficulty in adapting to high-end products, etc., to achieve enhanced hand feel, good application prospects and The effect of economic value
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] Preparation of finishing wax additive for water-based environment-friendly leather
[0020] 1) Weigh 100 parts of polyethylene wax (10 kg each), 96 parts of chlorinated paraffin, 100 parts of stearic acid, 100 parts of Span-60, 12 parts of skimmed milk powder, and 150 parts of silica matting powder; Homogenize the components and melt to a liquid state at 120±10°C;
[0021] 2) Put the melted composition described in step 1) into a reaction vessel containing 400 parts of deionized water, add 100 parts of Pingpingjia emulsifier that has been melted into a liquid state, and stir and emulsify at a constant speed for 20 to 30 minutes;
[0022] 3) Add 20 parts of preservative to the emulsified composition described in step 2), and cool it down to 35-40° C. to prepare the water-based environmental-friendly leather finishing matting wax additive.
Embodiment 2
[0024] Preparation of finishing wax additive for water-based environment-friendly leather
[0025] 1) Weigh 80 parts of polyethylene wax (10 kg each), 110 parts of chlorinated paraffin, 115 parts of stearic acid, 100 parts of Span-60, 15 parts of skimmed milk powder, and 130 parts of silica matting powder; Homogenize the components and melt to a liquid state at 120±10°C;
[0026] 2) Put the melted composition described in step 1) into a reaction vessel containing 500 parts of deionized water, add 95 parts of Pingpingjia emulsifier that has been melted into a liquid state, and stir and emulsify at a constant speed for 20 to 30 minutes;
[0027] 3) Add 20 parts of preservative to the emulsified composition described in step 2), and cool it to 35-40° C. to prepare the water-based paint matting wax additive for environment-friendly leather.
Embodiment 3
[0029] Water-based environmentally friendly leather finishing matting handle wax additives for artificial leather
[0030] Get 50 parts of water-based environment-friendly acrylic resin aqueous emulsion (every part 0.1kg), 100 parts of water-based environment-friendly polyurethane resin aqueous dispersions, 25 parts of water-based environment-friendly class leathers that embodiment 1 makes use finishing matting handle wax auxiliary agent, water-based metal complexing 20 parts of dyes (the water-based metal complex dyes are purchased from suppliers), 200 parts of pure water are stirred and mixed evenly, and the solid particles are filtered out with a 100-mesh filter screen to prepare sprayable water-based environmentally friendly leather with finishing matting handle wax. agent. Use 4kg / cm as water-based environmentally friendly leather finishing matting handle wax additive 2 The special spray gun is evenly sprayed on the surface of the artificial leather (such as PU leather) ...
PUM
| Property | Measurement | Unit |
|---|---|---|
| acid value | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More