Method for processing woolen knitted fabric
A technology of wool knitted fabrics and processing methods, which is applied in the fields of fabric surface trimming, textiles and papermaking, and dry-cleaning fiber products, etc., which can solve problems such as limitations in the field of use, and achieve the effect of overcoming loose tissue structure, elastic structure, and tight structure
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Embodiment one: the specific processing steps of getting the black pure wool double-sided jacquard fabric that is suitable for making an overcoat from 1 / 46NM black pure wool slubbed dyed yarn that the yarn count is:
[0017] (1) Black pure wool double-sided jacquard gray fabric is woven on a circular knitting machine with black pure wool slub dyed yarn with a yarn count of 1 / 46NM;
[0018] (2) Put the gray cloth into the overflow tank, control the weight bath ratio of wool gray cloth and water to 1:8, then add degreasing agent RC9 1.5g / L into the water, heat up to 50°C, keep warm for 20 minutes, and then drain. Rinse the gray cloth with clean water, then add water to the gray cloth again, control the weight-to-bath ratio of the gray cloth to water to 1:8, then add color-fixing agent TF-506 3g / L to the water, raise the temperature to 50°C and keep it warm for 20 minutes, and Drainage, dehydration;
[0019] (3) Add water to the softener, control the weight-to-bath ratio ...
Embodiment 2
[0028] Embodiment 2: The specific processing steps to process the wool double-sided jacquard fabric suitable for making coats are as follows:
[0029] (1) Take brown wool (70%) / acrylic (30%) blended gray yarn with a yarn count of 2 / 50NM and weave wool double-sided jacquard gray fabric on a circular knitting machine;
[0030] (2) Put the gray cloth into the overflow tank, control the weight bath ratio of wool gray cloth and water to 1:15, then add degreasing agent RC9 2g / L into the water, heat up to 60°C, keep warm for 30 minutes, drain, and use Rinse the gray cloth with clean water, then add water to the gray cloth again, control the weight-to-bath ratio of gray cloth and water to 1:10, then add color-fixing agent TF-506 1.5g / L to the water, raise the temperature to 60°C and keep it warm for 30 minutes, And drainage, dehydration;
[0031] (3) Add water to the softening machine, control the weight bath ratio of gray cloth to water to 1:15, then add softener IJD 8g / L to the wat...
Embodiment 3
[0040] Embodiment 3: The specific processing steps for processing a wool double-sided cloth suitable for making an overcoat from a wool (80%) / polyester (20%) blended gray yarn with a yarn count of 1 / 48NM are as follows:
[0041] (1) Take a yarn count of 1 / 48NM dark blue wool (80%) / polyester (20%) blended gray yarn on a circular knitting machine to weave wool double-sided gray fabric;
[0042](2) Put the gray cloth into the overflow tank, control the weight bath ratio of wool gray cloth and water to 1:10, then add degreasing agent RC9 1g / L into the water, heat up to 50°C, keep warm for 15 minutes, drain, and use Rinse the gray cloth with clean water, then add water to the gray cloth again, control the weight-to-bath ratio of gray cloth and water to 1:15, then add color-fixing agent TF-506 2g / L into the water, raise the temperature to 50°C, keep it warm for 15 minutes, and Drainage, dehydration;
[0043] (3) Add water to the softening machine, control the weight bath ratio of g...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com