Elastic wind sand/wear and corrosion/weather/temperature change resistant paint and preparation method thereof

A technology of sand resistance and abrasion resistance, applied in anti-corrosion coatings, polyurea/polyurethane coatings, coatings, etc., can solve the problems of poor high and low temperature deformation resistance, poor sand resistance, poor recovery rate, etc., and achieve excellent resistance to ultraviolet radiation. performance, improve construction efficiency, and facilitate construction

Active Publication Date: 2013-08-28
洛阳双瑞防腐工程技术有限公司
View PDF2 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The coating can solve the problems of poor weather resistance, poor durability, poor wind and sand resistance, poor wear resistance, poor recovery rate, poor high and low temperature deformation resistance, and difficult maintenance of outdoor material anticorrosion and protective coatings in the central and western regions of my country.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Elastic wind sand/wear and corrosion/weather/temperature change resistant paint and preparation method thereof
  • Elastic wind sand/wear and corrosion/weather/temperature change resistant paint and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0060] The composition and mass parts of component A are:

[0061] Rokrapol 2130:23.8

[0062] HGF: 17.9

[0063] Mixed solvent: 35.84

[0064] EFKA-5065: 0.36

[0065] TEGO-Foamex N: 0.12

[0066] MT-PLUS: 0.12

[0067] Tinuvin 900: 0.36

[0068] Nano slurry: 21.5

[0069] The composition and mass parts ratio of B component are:

[0070] Bayer-N75: 5

[0071] HDT-90: 95

[0072] A: B=5:1.

Embodiment 2

[0074] The composition and mass percentage of component A are:

[0075] Bayer VP LS 2971: 24.6

[0076] HGF: 19.0

[0077] Mixed solvent: 32.0

[0078] EFKA-4010: 0.7

[0079] TEGO-Foamex N: 0.5

[0080] Extra: 0.4

[0081] Tinuvin 900: 0.8

[0082] Homemade nano slurry: 22.0

[0083] The composition and mass percentage of component B are:

[0084] Bayer-N75: 7

[0085] Bayer-N3390: 93

[0086] A: B=4:1.

Embodiment 3

[0088] The composition and mass percentage of component A are:

[0089] Rokrapol 2130:30.0

[0090] HGF: 17.3

[0091] Mixed solvent: 31.0

[0092] EFKA-5065: 0.5

[0093] Deqian 6800: 0.3

[0094] MT-PLUS: 0.3

[0095] Hostavin ARO 8:0.6

[0096] Homemade nano slurry: 20.0

[0097] The composition and mass percentage of component B are:

[0098] Bayer-N75: 7

[0099] HDT-90: 93

[0100] A: B=7:1.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
particle diameteraaaaaaaaaa
hydroxyl valueaaaaaaaaaa
epoxy valueaaaaaaaaaa
Login to View More

Abstract

The invention discloses an elastic wind sand / wear and corrosion / weather / temperature change resistant paint. The paint comprises a component A and a component B, wherein the component A comprises 20.0-31.8 of elastic polyester resin, 15.0-20.0 of epoxy-organic silicone modified fluorocarbon resin, 30.0-33.0 of mixed solvent, 0.3-1.0 of wetting and dispersing agent, 0.1-0.5 of defoaming agent, 0.1-0.5 of thixotropic agent, 0.3-1.0 of ultraviolet complex stabilizer and 18.0-25.0 of nano slurry; and the component B comprises 5-10 of HDI (hexamethylenene diisocyanate) biuret and 90-95 of HDI tripolymer. The paint has the following advantages: the ultraviolet shielding rate of the paint can be more than 95%; the paint has excellent elasticity, wear resistance and recovery rate and can resist wind sand impact and high / low temperature deformation for a long time, and lives of the materials can reach 20 years after one-time coating; the paint has excellent self-cleaning and stain resisting functions; and the paint is convenient in construction and the one-time construction thickness can reach 150mu m.

Description

technical field [0001] The invention relates to an anti-corrosion coating technology, in particular to an elastic wind-sand, abrasion-resistant, weather-resistant and temperature-resistant coating and a preparation method thereof. Background technique [0002] Implementing the western development strategy and accelerating the economic development of the central and western regions is a major decision of our country to look far ahead, take the overall situation into consideration, and face the new century. It is a large-scale systematic project, and materials are the backbone of infrastructure construction and economic development in the central and western regions. and important foundations. Most of the central and western regions are dry and rainless areas (annual precipitation is below 150ml), strong and frequent sandstorms, strong ultraviolet radiation (more than 30% stronger than plain areas), and large temperature differences between day and night (-30°C to 60°C). Envi...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C09D175/06C09D7/12C09D5/08
Inventor 卫小星张东亚徐飞鹏刘翰锋
Owner 洛阳双瑞防腐工程技术有限公司