Tea aroma paper and preparation method thereof
A technology for tea fragrance and tea leaves, applied in the field of tea fragrance paper and its preparation, can solve problems such as monotonous color, and achieve the effect of improving added value and market competitiveness
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] The raw tea leaves are extracted with hot water at 90°C, and the solid-to-liquid ratio is controlled to be 1:5 by mass, and then the extract is concentrated to 50% solid content (mass) by a rotary evaporator at 70°C, and stored for later use .
[0022] Dilute polyvinyl alcohol with cold water to a mass concentration of 7.0%, soak for 4 hours, stir at a speed of 600r / min, then heat up to 95°C for boiling, keep warm for 2 hours, add water to dilute to 3% mass concentration, and store at 80°C insulation.
[0023] The extract that is 8% relative to the mass percentage of polyvinyl alcohol is mixed with polyvinyl alcohol solution to form a sizing material, and the solid content of the sizing material is 1%, and the sizing machine on the surface of the paper machine is used for sizing to obtain tea-flavored paper. The amount of glue is 2g / m 2 , the basis weight of the paper is 80g / m 2 , the mass content of tea extract in the paper is 0.2% (the percentage of tea extract = s...
Embodiment 2
[0026] The raw tea leaves were extracted with hot water at 95°C, with a solid-to-liquid ratio of 1:8 by mass, and then the extract was concentrated to 50% solid content by a rotary evaporator at 70°C, and stored for later use. Dilute polyvinyl alcohol with cold water to a mass concentration of 7.0%, soak for 4 hours, stir at a speed of 600r / min, then heat up to 95°C for boiling, keep warm for 2 hours, then dilute with water to a concentration of 2.5%, and keep warm at 75°C .
[0027] The extract that is 6% relative to the mass percentage of polyvinyl alcohol is mixed with polyvinyl alcohol solution to form a sizing material, the sizing material has a solid content of 1%, and sizing is carried out on a paper machine surface sizing machine to obtain tea-flavored paper. The amount of glue is 4g / m 2 , the basis weight of the paper is 40g / m 2 , the content of tea extract in the paper is 0.60% (the percentage of tea extract = sizing amount × extract and polyvinyl alcohol percentag...
Embodiment 3
[0029] The raw tea leaves were extracted with hot water at 90°C, with a solid-to-liquid ratio of 1:10, and then the extract was concentrated to 50% solid content by a rotary evaporator at 70°C, and stored for later use. Dilute polyvinyl alcohol with cold water to a mass concentration of 8.0%, soak for 4 hours, stir at a speed of 800r / min, then heat up to 95°C for boiling, keep warm for 2 hours, add water to dilute to 2.0% concentration, and keep warm at 70°C .
[0030] With respect to polyvinyl alcohol mass percentage is 10% extractant and polyvinyl alcohol solution are mixed and made into sizing material, and sizing material solid content is 1%, carries out sizing on paper machine surface sizing machine to obtain tea fragrance paper, sizing The amount of glue is 4g / m 2 , the basis weight of the copied paper is 40g / m 2 , the content of tea extract in the paper is 1% (the percentage of tea extract = sizing amount x extract and polyvinyl alcohol percentage ÷ quantitative x 100...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com