A technology of polyphenylene ring polyether succinate and polyphenylene ring polyether succinic acid, applied in the field of preparation of polyphenylene ring polyether succinate and its sulfonate, can solve the overall performance gap and stability over time Problems such as delamination phenomenon and polyphenylene ring polyether modification have not been reported, so as to achieve the effect of improving various properties
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] Example 1: Add polyphenylene ring polyether (triphenylethylphenol polyether, molecular weight 2000-2500) and maleic anhydride into the reactor at a molar ratio of 1:1, start stirring, and the esterification temperature is 80-100°C. °C without catalyst, react under nitrogen protection conditions for 4 hours to obtain polyphenyl ring polyether succinate, then add sulfonating agent (sulfuric acid) and react at 100-170 °C for 3-4 hours to obtain the finished product: polyphenyl ring Polyether succinate sulfonate.
Embodiment 2
[0026] Example 2: Add polyphenylene ring polyether (triphenylethylphenol polyether, molecular weight 2000-2500) and maleic anhydride into the reactor at a molar ratio of 1:1, start stirring, and the esterification temperature is 80-100°C , without a catalyst, reacted for 4 hours under the condition of nitrogen protection, and then added an equiproportional mole of polyphenylene ring polyether to the reactor. Until very few, add sulfonating agent (fuming sulfuric acid) into the reaction kettle, react at 100-170°C for 3-4 hours, and obtain the finished product: polyphenylene ring polyether succinate sulfonate.
Embodiment 3
[0027] Example 3: Add polyphenylene ring polyether (triphenylethylphenol polyether, molecular weight 1500-2000) and maleic anhydride in a molar ratio of 1:1 into the reactor, start stirring, and the esterification temperature is 80-100°C. Without catalyst, react under nitrogen protection for 4 hours to obtain polyphenylene ring polyether succinate, then add sulfonating agent (sulfamic acid) and react at 100-170 °C for 3-4 hours to obtain the finished product: benzene ring polyether succinate Ether succinate sulfonate.