Embodiment 1
[0022] Refer to the attached figure 1 , to describe Embodiment 1 of the present invention in detail.
[0023] Raw material: A sample of a copper-nickel sulfide mining area in Jinchuan, Gansu, its main chemical composition is (%)
[0024] Ni
Cu
MgO
1.41
1.01
27.48
[0025] One or several of xanthate, butyl xanthate, pentaxanthate, Y89-2 xanthate, etc. are used as collectors, sodium carbonate is used as pH regulator, metaphosphate, polyphosphate, water glass One or several of them, such as organic polymers, are used as regulators for froth flotation.
[0026] The process is: grind the ore to -0.074mm, accounting for 65%, add collector Y89-2 xanthate, carry out mechanical stirring and dispersing treatment under the stirring intensity of 2800r / min for 20min, and feed it into the flotation equipment for roughing two For the first sweeping operation, 150g / t of regulator sodium hexametaphosphate was added to the coarse concentrate for dispers...
Embodiment 2
[0032] Refer to the attached figure 2 , to describe Embodiment 2 of the present invention in detail.
[0033] Raw material: A sample of a copper-nickel sulfide mining area in Jinchuan, Gansu, its main chemical composition is (%)
[0034] Ni
Cu
MgO
1.35
0.97
25.93
[0035] Other conditions are with embodiment 1.
[0036] The process is as follows: take a slurry sample with a grinding fineness of -0.074mm, accounting for 66%, add regulator sodium hexametaphosphate, collector butyl xanthate, mechanically stir and disperse for 40 minutes at a stirring intensity of 2500r / min, and feed The flotation equipment performs one roughing and two sweeping operations; add 700g / t regulator sodium hexametaphosphate to the rough concentrate obtained by roughing, and perform two beneficiation to obtain concentrate 1; the second beneficiation of middle ore Concentrate 2 is obtained by concentration; the tailings obtained after two sweeps are screened at ...
Embodiment 3
[0041] Refer to the attached image 3 , to describe Embodiment 3 of the present invention in detail.
[0042] Raw material: A sample of a copper-nickel sulfide mining area in Jinchuan, Gansu, its main chemical composition is (%)
[0043] Ni
Cu
MgO
1.43
1.09
26.37
[0044] Other conditions are with embodiment 1.
[0045] The process is as follows: take a slurry sample with a grinding fineness of -0.074mm, accounting for 65%, add the collector butyl xanthate, and mechanically stir and disperse for 20 minutes under the condition of 2500r / min stirring intensity, and then feed it into the flotation equipment for a rough separation , the regulator sodium hexametaphosphate and ultrasonic waves are added to the coarse concentrate pulp for dispersion treatment, a beneficiation is carried out, and then sodium hexametaphosphate is added for dispersion treatment and then the second beneficiation is carried out to obtain the final concentrate.
[0...