Preparation method of softening agent for hard and dry leather cultural relics
A technology for leather and cultural relics, applied in the field of softening agent preparation, can solve the problems of leather cultural relics aging, cultural relics damage, cracking, etc., and achieve obvious effects, increased softness, and strong pertinence
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0015] Embodiment 1: a kind of softening agent preparation method for dry hard leather cultural relics, comprises the following steps:
[0016] 1) Add lactic acid solution with a volume fraction of 75% to natural phospholipids, and the amount of lactic acid solution is 1% of the mass of natural phospholipids;
[0017] 2) Heat the above mixed liquid in a water bath while stirring, the time is 2 hours, and the temperature is 65°C;
[0018] 3) Within the first 30 minutes of the above heating and stirring process, gradually add hydrogen peroxide solution with a mass fraction of 30%, and the amount of hydrogen peroxide solution is 15% of the mass of natural phospholipids;
[0019] 4) After the above-mentioned heating and stirring process is completed, the mixed liquid is titrated to neutrality with a sodium hydroxide solution having a mass fraction of 5%, and then the mixed liquid is vacuum-dried to obtain a hydroxylated modified phospholipid;
[0020] 5) Compound the above-mentio...
Embodiment 2
[0021] Embodiment 2: a kind of softening agent preparation method for dry hard leather cultural relics, comprises the following steps:
[0022] 1) Add lactic acid solution with a volume fraction of 75% to natural phospholipids, and the amount of lactic acid solution is 2% of the mass of natural phospholipids;
[0023] 2) Heat the above mixed liquid in a water bath while stirring, the time is 1h, and the temperature is 70°C;
[0024] 3) Within the first 30 minutes of the above heating and stirring process, gradually add hydrogen peroxide solution with a mass fraction of 30%, and the amount of hydrogen peroxide solution is 5% of the mass of natural phospholipids;
[0025] 4) After the above-mentioned heating and stirring process is completed, the mixed liquid is titrated to neutrality with a sodium hydroxide solution having a mass fraction of 5%, and then the mixed liquid is vacuum-dried to obtain a hydroxylated modified phospholipid;
[0026] 5) Compound the above-mentioned hy...
Embodiment 3
[0027] Embodiment 3: a kind of softening agent preparation method for dry hard leather cultural relics, comprises the following steps:
[0028] 1) Add lactic acid solution with a volume fraction of 75% to natural phospholipids, and the amount of lactic acid solution is 3% of the mass of natural phospholipids;
[0029] 2) Heat the above mixed liquid in a water bath while stirring for 3 hours at a temperature of 50°C;
[0030] 3) Within the first 30 minutes of the above heating and stirring process, gradually add hydrogen peroxide solution with a mass fraction of 30%, and the amount of hydrogen peroxide solution is 10% of the mass of natural phospholipids;
[0031] 4) After the above-mentioned heating and stirring process is completed, the mixed liquid is titrated to neutrality with a sodium hydroxide solution having a mass fraction of 5%, and then the mixed liquid is vacuum-dried to obtain a hydroxylated modified phospholipid;
[0032] 5) Compound the above-mentioned hydroxyla...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.