Embodiment 1
[0017] A dyeing and finishing process of wool and recycled polyester blended fabrics, comprising the steps of:
[0018] 1) Desizing: add 4g / L chelating dispersant, 1g / L wax remover, 8g / L desizing enzyme, 6g / L refining agent;
[0019] 2) Bleaching: add 3g / L tribasic lead sulfate, 8g / L hydrogen peroxide;
[0020] 3) Set the shape at 220°C for 1 minute;
[0021] 4) Dyeing: add water, the bath ratio is 2:7, put the fabric into operation for 5 minutes, add dyeing auxiliaries, acetic acid and disperse dyes in sequence, adjust the pH value to 3.5, and heat up to 110°C at 5°C / min , keep warm for 40 minutes, cool down to 30°C at 5°C / min, wash and drain;
[0022] Add water, the bath ratio is 3:11, run for 5 minutes, add dyeing auxiliaries and acid dyes in turn, run for 15 minutes, heat up to 90°C at 5°C / min, keep warm for 30 minutes, cool down to 70°C at 5°C / min , washing and draining;
[0023] Add water, the bath ratio is 2:7, add 5g / L soaping agent, heat to 85°C, keep warm for 40 ...
Embodiment 2
[0027] A dyeing and finishing process of wool and recycled polyester blended fabrics, comprising the steps of:
[0028] 1) Desizing: add 6g / L chelating dispersant, 2g / L wax remover, 9g / L desizing enzyme, 7g / L refining agent;
[0029] 2) Bleaching: add 4g / L tribasic lead sulfate, 9g / L hydrogen peroxide;
[0030] 3) Set the shape at 220°C for 1 minute;
[0031] 4) Dyeing: add water, the bath ratio is 2:7, put the fabric into operation for 5 minutes, add dyeing auxiliaries, acetic acid and disperse dyes in sequence, adjust the pH value to 3.5, and heat up to 110°C at 5°C / min , keep warm for 40 minutes, cool down to 30°C at 5°C / min, wash and drain;
[0032] Add water, the bath ratio is 3:11, run for 5 minutes, add dyeing auxiliaries and acid dyes in turn, run for 15 minutes, heat up to 90°C at 5°C / min, keep warm for 30 minutes, cool down to 70°C at 5°C / min , washing and draining;
[0033] Add water, the bath ratio is 2:7, add 5g / L soaping agent, heat to 85°C, keep warm for 40 ...
Embodiment 3
[0037] A dyeing and finishing process of wool and recycled polyester blended fabrics, comprising the steps of:
[0038] 1) Desizing: add 4.6g / L chelating dispersant, 1.2g / L wax remover, 8.9g / L desizing enzyme, 6.7g / L refining agent;
[0039] 2) Bleaching: Add 3.4g / L tribasic lead sulfate and 8.9g / L hydrogen peroxide;
[0040] 3) Set the shape at 220°C for 1 minute;
[0041] 4) Dyeing: add water, the bath ratio is 2:7, put the fabric into operation for 5 minutes, add dyeing auxiliaries, acetic acid and disperse dyes in sequence, adjust the pH value to 3.5, and heat up to 110°C at 5°C / min , keep warm for 40 minutes, cool down to 30°C at 5°C / min, wash and drain;
[0042] Add water, the bath ratio is 3:11, run for 5 minutes, add dyeing auxiliaries and acid dyes in turn, run for 15 minutes, heat up to 90°C at 5°C / min, keep warm for 30 minutes, cool down to 70°C at 5°C / min , washing and draining;
[0043] Add water, the bath ratio is 2:7, add 5g / L soaping agent, heat to 85°C, ke...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com