A kind of antistatic fabric and weaving method
An anti-static and manufacturing method technology, applied in the field of anti-static fabric weaving, anti-static fabric and weaving, can solve the problems of affecting anti-static property, less variety of colors, not enough soft hand feeling, etc., and achieve excellent anti-static performance and excellent textile performance. , Comfortable and breathable
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0020] 1. Put the blended fabric into a 20g / L sodium hydroxide alkali tank, and perform alkali reduction treatment, so that the weight ratio of the blended fabric to the alkali solution is 1:50, and treat it at 60°C for 75 minutes, and cool it after treatment to room temperature, neutralized to pH 7 with 2% acetic acid solution, rinsed with water and dried at 60°C for later use;
[0021] 2. To prepare the solution, take 50ml of 0.04mol / L zinc nitrate solution and add 50ml of 0.08mol / L amino-containing alkali solution, stir vigorously at 400rpm for 2 hours, and keep the temperature of the prepared solution at 60-95°C;
[0022] 3. Add the spare blended fabric fabric prepared by step ① into the container containing the solution prepared in step ②, and add 0.4g of polyvinylpyrrolidone and 50ml of ethanol with a concentration of 95% to it at the same time, and then place it in 35KHz frequency ultrasonic After processing for 15 minutes, take out the blended fabric and dry it, then i...
Embodiment 2
[0025] 1. Put the cotton fabric into a 30g / L ammonia water alkali tank, so that the weight ratio of the cotton fabric to the alkali solution is 1:50, and treat it for 105 minutes at 100°C, cool to room temperature after treatment, and use a concentration of 5% acetic acid solution to neutralize to pH 10, wash with water and dry at 60°C for later use;
[0026] 2. To prepare the solution, take 50ml of 0.12mol / L zinc chloride solution and add 50ml of 0.15mol / L amino-containing alkaline solution, stir vigorously at 1000rpm for 2 hours, and keep the temperature of the prepared solution at 95°C;
[0027] 3. Add the spare cotton fabric fabric prepared through step 1 to the container containing the solution prepared in step 2, and add 0.4 g of polyethylene glycol and 50 ml of methanol at a concentration of 95% to it, and then place it in a 35KHz frequency ultrasonic Treat for 15 minutes, take out the cotton fabric and immerse the cotton fabric again after drying;
[0028] 4. Finally,...
Embodiment 3
[0030] 1. Put the woolen fabric into a 25g / L urea alkali tank for treatment, so that the weight ratio of the woolen fabric to the alkali solution is 1:50, treat at 80°C for 90 minutes, cool to room temperature after treatment, and use 3% urea Neutralize pH to 9 with acetic acid solution, wash with water and dry at 60°C for later use;
[0031] 2. To prepare the solution, take 50ml of 0.08mol / L zinc acetate solution and add 50ml of 0.12mol / L amino-containing alkali solution, stir vigorously at 600rpm for 2 hours, and keep the temperature of the prepared solution at 80°C;
[0032] 3. Add the standby woolen fabric fabric prepared by step ① into the container containing the solution prepared in step ②, and add 0.4g of polyethylene glycol and 50ml of ethanol with a concentration of 95% to it at the same time, and then place it in 35KHz frequency ultrasonic Treat for 15 minutes, take out the woolen fabric and immerse the woolen fabric again after drying;
[0033] 4. Finally, dry the...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More 