A kind of wall coating and preparation method thereof
A paint and wall technology, applied in the field of wall paint and preparation, can solve the problems of high production cost, easy mold on the wall, poor environmental protection performance, etc., and achieve the effect of low production cost, good covering effect and low cost
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Publication Date
- 2016-07-06
Smart Images
Figure 1 Figure 2
Abstract
Description
technical field
[0001] The invention belongs to the technical field of coatings, and in particular relates to a wall coating and a preparation method. Background technique
[0002] Coatings play an important role in the national economy and are indispensable in modern society. However, there are more than 10 million tons of volatile organic compounds (VOC) emitted into the atmosphere from paints in the world every year, which is one of the main sources of air pollution. At present, the existing wall paints are usually easy to use during use. The following problems occur: it contains certain harmful substances such as formaldehyde and volatile organic compounds, and usually emits an unpleasant smell for a long time, and the environmental performance is poor, which brings lasting harm to people's bodies. Consumers bring a lot of inconvenience.
[0003] There are also some green paints on the market at present, but the production cost is high and cannot meet the huge market d...
Examples
Embodiment 1
[0025] It is characterized in that the coating consists of the following components by weight:
[0026] Weigh 15kg of bamboo pulp, 30kg of straw pulp, and 15kg of rag pulp, mix them evenly, break them with a beater, add 300kg of water, dilute them and put them in the reaction kettle, add 1.5kg of defoamer, at a speed of 700-900 rpm Stir for 15 minutes under the condition of high temperature; then add 100kg of titanium dioxide, 230kg of pure acrylic acid emulsion, and stir for 20-30 minutes at the speed of 500-1200 rpm, and sand mill until the fineness of the material is below 50um; Put 35kg of vegetable gum composition, 1.5kg of defoamer, and 4kg of plant extract into the reactor, and stir for 15-30 minutes at a speed of 400-800 rpm; finally adjust with 1.5kg of high-alkalinity compound alkali When the pH value reaches 6-7, it is a qualified product after passing through a 200-mesh sieve, and it is packaged and stored.
[0027] Preparation of the vegetable gum composition: We...
Embodiment 2
[0030] Weigh 15kg of bamboo pulp, 30kg of straw pulp, and 15kg of rag pulp, mix them evenly, break them with a beater, add 300kg of water, dilute them and put them in the reaction kettle, add 1.5kg of defoamer, at a speed of 700-900 rpm Stir for 15 minutes under the conditions; then add 100kg of titanium dioxide and 230kg of polyvinyl acetate latex, stir for 20-30 minutes at a speed of 500-1200 rpm, and sand-mill until the fineness of the material is below 50um ; 35kg vegetable gum composition, 1.5kg defoamer, 4kg plant extract to the reactor, stirring for 15-30 minutes under the condition of 400-800 rpm at a rotating speed; finally use 1.5kg of high alkalinity compound alkali Adjust the pH value to 6-7, and pass through a 200-mesh sieve to be a qualified product, which is packaged and stored.
[0031] Preparation of the vegetable gum composition: Weigh 35 kg of cougar gum and 35 kg of stone flower gum, and mix the two to obtain the vegetable gum composition. Among them, coum...
Embodiment 3
[0034] Weigh 10kg of bamboo pulp, 20kg of straw pulp, and 10kg of rag pulp, mix them evenly, smash them with a beater, add 200kg of water to dilute them, put them into the reaction kettle, add 1kg of defoamer, and mix them at a speed of 700-900 rpm Stir at high temperature for 15 minutes; then add 70kg of titanium dioxide, 180kg of pure acrylic emulsion, and stir for 20-30 minutes at a speed of 500-1200 rpm, and sand mill until the material fineness is below 50um; 30kg of plant Put the glue composition, 1kg defoamer, and 2kg plant extract into the reactor, and stir for 15-30 minutes at a speed of 400-800 rpm; finally adjust the pH value to 6 with 1kg of high-alkalinity compound base -7. After passing through a 200-mesh sieve, it is a qualified product, which is packaged and preserved.
[0035] Preparation of vegetable gum composition: Weigh 30 kg of coriander gum and 30 kg of stone flower gum, and mix the two to obtain the vegetable gum composition. Among them, coumarin gum a...