A technology of viscose fiber and viscose staple fiber, which is applied in the field of functional viscose fiber and its preparation, can solve the problems of poor permeability and air permeability of synthetic fibers, complicated process, and influence on human comfort, and achieve good preventability , The effect of simple process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0028] The production method of embodiment 1 cotton type diatom base viscose staple fiber
[0029] A. Prepare diatom-based powder liquid slurry according to the following ratio
[0030] Ultrafine diatom-based powder 20%
[0031] Water-soluble dispersant 1% TLT-540I type (Guangzhou Tolite Chemical Co., Ltd.)
[0032] Distilled water 79%
[0033] Stir the above components evenly, among which the diatomite powder with a particle size of less than 0.5 μm of diatom-based powder accounts for more than 60%, the average particle size is less than 0.65 μm, and the dispersion degree is greater than 80%.
[0034] B. Preparation of diatom-based viscose fiber
[0035] Follow these steps:
[0036] Alkalinization, yellowing, dissolution, primary filtration, ripening, defoaming, secondary filtration, wet spinning, coagulation, plasticizing and drawing, cutting, post-processing, drying and packaging of cellulose A;
[0037] Among them: the input amount of each batch of A cellulose (pulp) ...
Embodiment 2
[0041] Embodiment 2. Preparation of filament diatom-based viscose fiber
[0042] A. Prepare diatom-based powder liquid slurry according to the following ratio
[0043] Ultrafine diatom-based powder 22%
[0044] Water-soluble dispersant 2%
[0045] Distilled water 76%
[0046] Stir the above components evenly, among which the diatomite powder with a particle size of less than 0.5 μm of diatom-based powder accounts for more than 60%, the average particle size is less than 0.65 μm, and the dispersion degree is greater than 80%.
[0047] B. Preparation of diatom-based viscose fiber
[0048] Follow these steps:
[0049] Type A cellulose impregnation, pressing, yellowing, dissolving, primary filtration, aging, secondary filtration, ripening, defoaming, tertiary filtration, wet spinning, post-treatment and barrel forming;
[0050] Wherein: after filtering three times, add the prepared diatom-based powder liquid slurry, the addition amount is 2.9% of the total mass percentage of ...
Embodiment 3
[0053] The preparation of embodiment 3 cotton-type diatom-based viscose short fibers
[0054] A. Prepare diatom-based powder liquid slurry according to the following ratio
[0055] Ultrafine diatom-based powder 30%
[0056] Water-soluble dispersant 2% TLT-540I type (Guangzhou Tolite Chemical Co., Ltd.)
[0057] Distilled water 68%
[0058] Stir the above components evenly, among which the diatomite powder with a particle size of less than 0.5 μm accounts for more than 80%, the average particle size is less than 0.65 μm, and the dispersion degree is greater than 80%.
[0059] B. Preparation of diatom-based viscose fiber
[0060] Follow these steps:
[0061] Alkalinization, yellowing, dissolution, primary filtration, ripening, defoaming, secondary filtration, wet spinning, coagulation, plasticizing, drawing, cutting, post-processing, drying and packaging of cellulose A;
[0062] Among them: the input amount of each batch of A cellulose (pulp) is 450kg, in the alkalization s...
PUM
Property | Measurement | Unit |
---|---|---|
particle size | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology