Spray paint for outside surfaces of motors and preparation method thereof
A technology of external surface and chlorinated rubber, which is applied in coatings, anti-corrosion coatings, polyurea/polyurethane coatings, etc., can solve problems such as poor adhesion, short adhesion time, and low adhesion strength, and achieve extended service life and good protection function, the effect of excellent adhesion
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A spray paint for the outer surface of a motor, comprising the following raw materials in parts by mass: 15 parts of linseed oil, 15 parts of trimethylolpropane, 15 parts of methyl diisocyanate, 2 parts of sorbic acid, 2 parts of phthalic anhydride, dioxin 0.7 parts of alkanes, 0.01 parts of ethyl cellosolve, 2 parts of aluminum silver paste, 2 parts of oxalic acid, 2 parts of benzoyl peroxide, 3 parts of cobalt naphthenate, 0.5 parts of sodium peroxide, 6 parts of chlorinated rubber .
[0019] A preparation method for spraying paint on the outer surface of a motor, comprising the steps of:
[0020] Step 1: Mix and stir linseed oil, trimethylolpropane and ethyl cellosolve evenly, heat to 200°C, keep warm for 2 hours, cool to 140°C, add methyl diisocyanate and mix, heat at 180°C for 4 hours, Cool to 70°C, add sorbic acid, dioxane and phthalic anhydride, mix evenly, heat to 160°C within 1.5h, keep warm for 1.5h to obtain a copolymer;
[0021] The second step: dissolve t...
Embodiment 2
[0023] A spray paint for the outer surface of a motor, comprising the following raw materials in parts by mass: 27 parts of linseed oil, 25 parts of trimethylolpropane, 27 parts of methyl diisocyanate, 5.5 parts of sorbic acid, 5.5 parts of phthalic anhydride, dioxin 2.5 parts of alkanes, 0.03 parts of ethyl cellosolve, 5 parts of aluminum silver paste, 4 parts of oxalic acid, 4.5 parts of benzoyl peroxide, 6 parts of cobalt naphthenate, 1 part of sodium peroxide, 15 parts of chlorinated rubber .
[0024] A preparation method for spraying paint on the outer surface of a motor, comprising the steps of:
[0025] Step 1: Mix and stir linseed oil, trimethylolpropane and ethyl cellosolve evenly, heat to 240°C, keep warm for 3h, cool to 160°C, add methyl diisocyanate and mix, heat at 200°C for 5h, Cool to 90°C, add sorbic acid, dioxane and phthalic anhydride, mix well, heat to 180°C within 2.5 hours, keep warm for 2.5 hours to obtain a copolymer;
[0026] The second step: dissolve...
Embodiment 3
[0028] A spray paint for the outer surface of a motor, comprising the following raw materials in parts by mass: 18 parts of linseed oil, 18 parts of trimethylolpropane, 17 parts of methyl diisocyanate, 3 parts of sorbic acid, 3 parts of phthalic anhydride, dioxin 1 part alkanes, 0.015 parts ethyl cellosolve, 3 parts aluminum silver paste, 2.5 parts oxalic acid, 2.5 parts benzoyl peroxide, 3.5 parts cobalt naphthenate, 0.6 parts sodium peroxide, 8 parts chlorinated rubber .
[0029] A preparation method for spraying paint on the outer surface of a motor, comprising the steps of:
[0030] Step 1: Mix and stir linseed oil, trimethylolpropane and ethyl cellosolve evenly, heat to 200°C, keep warm for 2 hours, cool to 140°C, add methyl diisocyanate and mix, heat at 180°C for 4 hours, Cool to 70°C, add sorbic acid, dioxane and phthalic anhydride, mix evenly, heat to 160°C within 1.5h, keep warm for 1.5h to obtain a copolymer;
[0031] The second step: dissolve the aluminum silver p...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com