All-cotton easy-care shirt processing method
A processing method and shirt technology, which is applied in the field of cotton non-ironing shirt processing, can solve problems such as environmental pollution and adverse effects on human health, and achieve the effects of strong operability, saving water and electricity energy consumption, and high air permeability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0027] In the embodiment of the present invention, a method for processing a cotton non-iron shirt includes the following steps:
[0028] 1) Cutting: After the cotton fabric is typeset and cut, the edge of the cotton fabric is shaped by a partial coating process with a low-viscosity stiffener as the coating finishing agent;
[0029] 2) Sewing: Sewing the cut fabric to obtain a semi-finished shirt;
[0030] 3) Atomized spray: The raw materials of the finishing solution in terms of mass percentage include 18% modified dihydroxymethyldihydroxyethylene urea, 2.2% zinc chloride, 2.5% amino silicone oil, 1% polyethylene, 20% formaldehyde scavenger and Adjust the pH value of the finishing liquid to 4.0 by adding glacial acetic acid to 56.3% water; spray the finishing liquid onto the sewn shirt using an atomization device to make the shirt liquid rate 70%; specifically including the following steps:
[0031] Spraying, the pressure is 2kg / cm 2 , The rotation speed of the atomization device is ...
Embodiment 2
[0040] In the embodiment of the present invention, a method for processing a cotton non-iron shirt includes the following steps:
[0041] 1) Cutting: After typesetting and cutting the cotton fabric, use a local coating process with a low-viscosity stiffener as the coating finishing agent to shape the edge of the cotton fabric;
[0042] 2) Sewing: Sewing the cut fabric to obtain a semi-finished shirt;
[0043] 3) Atomized spray: The raw materials of the finishing liquid in terms of mass percentage include modified dihydroxymethyldihydroxyethylene urea 23%, zinc nitrate 2%, amino silicone oil 3.5%, polyethylene 1.5%, formaldehyde scavenger 30% and water 40%, adjust the pH of the finishing liquid to 4.5 by adding glacial acetic acid; spray the finishing liquid onto the sewn shirt by using an atomizing device to make the shirt liquid rate 80%; specifically include the following steps:
[0044] Spraying, the pressure is 2.5kg / cm 2 , The rotation speed of the atomization device is 25r / min, ...
Embodiment 3
[0053] In an embodiment of the present invention, a method for processing a cotton non-iron shirt includes the following steps:
[0054] 1) Cutting: After typesetting and cutting the cotton fabric, use a local coating process with a low-viscosity stiffener as the coating finishing agent to shape the edge of the cotton fabric;
[0055] 2) Sewing: Sewing the cut fabric to obtain a semi-finished shirt;
[0056] 3) Atomized spray: The raw materials of the finishing solution in terms of mass percentage include modified alkyl dihydroxy ethylene urea 20%, magnesium chloride 2.2%, amino silicone oil 3%, polyethylene 0.5%, formaldehyde scavenger 25% and water 49.3%, Adjust the pH value of the finishing liquid to 4.0 by adding glacial acetic acid; spray the finishing liquid onto the sewn shirt with an atomizing device to make the shirt liquid rate 70%; specifically including the following steps:
[0057] Spraying, the pressure is 2.5kg / cm 2 , The rotation speed of the atomization device is 25r / ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com