A kind of non-woven fabric containing photocatalyst and its formula and preparation method
A technology of photocatalyst and non-woven fabrics, applied in the direction of non-woven fabrics, textiles, papermaking, fiber types, etc., can solve problems such as air pollution, deodorization, self-cleaning and air purification functions cannot be satisfied, environmental pollution, etc., to achieve release Long-lasting, long-lasting sterilization and purification function, and the effect of removing formaldehyde
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0014] Viscose fiber: 210kg / t, polyester fiber: 490kg / t, styrene-acrylate crosslinking emulsion: 410kg / t, pure acrylate self-crosslinking emulsion: 136kg / t, photocatalyst titanium dioxide dispersion: 180kg / t, hair Foaming agent K-12: 3kg / t.
[0015] Viscose 1.5D*38MM: 30%;
[0016] Polyester 1.5D*38MM: 70%;
[0017] Styrene-acrylate cross-linked emulsion (anionic, solid content 50%, Tg=-30℃, viscosity<300 cps);
[0018] Pure acrylate self-crosslinking emulsion (anionic, solid content 55%, Tg=3°C, viscosity <300 cps,);
[0019] The solid content of photocatalyst titanium dioxide dispersion liquid is 10%;: (supplier: Shanghai Jianghu Titanium White Chemical Products Co., Ltd.).
[0020] The polyester and viscose fibers are opened and carded, formed into a net, foam sizing and photocatalyst, and then dried and wound.
Embodiment 2
[0022] Viscose fiber: 220kg / t, polyester fiber: 510kg / t, styrene-acrylate crosslinking emulsion: 430kg / t, pure acrylate self-crosslinking emulsion: 145kg / t, photocatalyst titanium dioxide dispersion: 190 kg / t, Foaming agent K-12: 4kg / t.
[0023] Viscose 1.5D*38MM: 30%;
[0024] Polyester 1.5D*38MM: 70%;
[0025] Styrene-acrylate cross-linked emulsion (anionic, solid content 50%, Tg=-30℃, viscosity<300 cps);
[0026] Pure acrylate self-crosslinking emulsion (anionic, solid content 55%, Tg=3°C, viscosity <300 cps,);
[0027] The solid content of photocatalyst titanium dioxide dispersion liquid is 10%;: (supplier: Shanghai Jianghu Titanium White Chemical Products Co., Ltd.).
[0028] The polyester and viscose fibers are opened and carded, formed into a net, foam sizing and photocatalyst, and then dried and wound.
Embodiment 3
[0030] Viscose fiber: 230kg / t, polyester fiber: 540kg / t, styrene-acrylate crosslinking emulsion: 450kg / t, pure acrylate self-crosslinking emulsion: 150kg / t, photocatalyst titanium dioxide dispersion: 200 kg / t, Foaming agent K-12: 5kg / t.
[0031] Viscose 1.5D*38MM: 30%;
[0032] Polyester 1.5D*38MM: 70%;
[0033] Styrene-acrylate cross-linked emulsion (anionic, solid content 50%, Tg=-30℃, viscosity<300 cps);
[0034] Pure acrylate self-crosslinking emulsion (anionic, solid content 55%, Tg=3°C, viscosity <300 cps,);
[0035] The solid content of photocatalyst titanium dioxide dispersion liquid is 10%;: (supplier: Shanghai Jianghu Titanium White Chemical Products Co., Ltd.).
[0036] The polyester and viscose fibers are opened and carded, formed into a net, foam sizing and photocatalyst, and then dried and wound.
[0037] The non-woven fabric index prepared by the formula of the present invention:
[0038] Gram weight: 30+-2g / ㎡; feel: soft
[0039] Width: 1.00M (or cut as r...
PUM
| Property | Measurement | Unit |
|---|---|---|
| solid content | aaaaa | aaaaa |
| solid content | aaaaa | aaaaa |
| purity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
Login to View More 