Method for improving leather softness synergistically by using acid proteinase
An acid protease, softness technology, applied in application, leather impregnation, leather surface treatment, etc., can solve the problems of no synergistic effect of enzyme treatment auxiliaries, no report on enzyme application research, etc., to achieve sustainable development. , Improve the softness, the effect of being conducive to environmental protection
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A method for synergistically improving leather softness by applying acid protease, comprising the following steps:
[0019] (1) Weighing: chrome-tanned sheep leather (blue leather) is weighed as a benchmark for subsequent operations.
[0020] (2) Add water in the drum according to the liquid ratio of 1.5, adjust the pH value to 5.0, and the temperature is 40°C, put in chrome tanned leather, transfer to the drum, and fully rehydrate.
[0021] (3) Add 6% acid protease and 6% amino silicone oil, and rotate for 6 h.
[0022] (4) Formic acid fixation: adjust the pH to 4.0~4.5 with formic acid, remove the drum, and ride the horse.
Embodiment 2
[0024] A method for synergistically improving leather softness by applying acid protease, comprising the following steps:
[0025] (1) Weighing: chrome-tanned sheep leather (blue leather) is weighed as a benchmark for subsequent operations.
[0026] (2) Add water in the drum according to the liquid ratio of 1.5, adjust the pH value to 5.0, and the temperature is 40°C, put in chrome tanned leather, transfer to the drum, and fully rehydrate.
[0027] (3) Add 6% acid protease and 6% polyether silicone oil, and rotate for 6 h.
[0028] (4) Formic acid fixation: adjust the pH to 4.0~4.5 with formic acid, remove the drum, and ride the horse.
Embodiment 3
[0030] A method for synergistically improving leather softness by applying acid protease, comprising the following steps:
[0031] (1) Weighing: Zirconium-aluminum-titanium chrome-free multi-metal tanned sheep leather is weighed as a benchmark for subsequent operations.
[0032] (2) Add water in the drum according to the liquid ratio of 1.5, adjust the pH value to 5.0, and the temperature is 40°C, put in chrome tanned leather, transfer to the drum, and fully rehydrate.
[0033] (3) Add 6% acid protease and 6% amino silicone oil, and rotate for 6 h.
[0034] (4) Formic acid fixation: adjust the pH to 4.0~4.5 with formic acid, remove the drum, and ride the horse.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com