Formaldehyde-removing antibacterial seaweed mud paint and preparation method thereof
A technology of seaweed mud and aldehyde purification, applied in the field of decorative materials, can solve the problems of inability to decompose formaldehyde, insufficient antibacterial and antifungal effects, rough hand feeling of paint film, etc. Smooth and delicate paint film surface
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0029] The net aldehyde antibacterial seaweed mud paint of the present embodiment comprises 25 parts of water, 0.6 part of dispersant, 1.0 part of antifreeze, 1.2 parts of film-forming aids, 15 parts of titanium dioxide, 18 parts of calcium carbonate, 6 parts according to parts by weight. Kaolin, 5 parts of mica powder, 0.2 parts of nano-silver antibacterial agent, 5 parts of seaweed mud, 0.4 parts of thickener, 0.5 parts of negative ion additives, 20 parts of deodorant lotion, 0.2 parts of antifungal agent, 0.25 parts of preservative and 0.15 parts of hydrophobic agent.
[0030] Prepare as follows:
[0031] (1) Pre-mixing: Add 2 / 3 of water to the dispersion tank, add dispersant, anion additive and thickener, and mix at 600rpm for 8 minutes;
[0032] (2) Grinding and dispersing: Add seaweed mud at a speed of 1200rpm, increase the speed to 2200rpm and disperse for 8min, then reduce the speed to 1200rpm, put in titanium dioxide, kaolin, mica powder and calcium carbonate, and di...
Embodiment 2
[0036] The net aldehyde antibacterial seaweed mud paint of the present embodiment comprises 28 parts of water, 0.7 part of dispersing agent, 1.0 part of antifreeze, 1.0 part of film-forming aid, 20 parts of titanium dioxide, 16 parts of calcium carbonate, 7 parts according to parts by weight. Kaolin, 4 parts of mica powder, 0.25 parts of nano-silver antibacterial agent, 6 parts of seaweed mud, 0.4 parts of thickener, 0.6 parts of negative ion additives, 25 parts of deodorizing emulsion, 0.25 parts of antifungal agent, 0.25 parts of preservative and 0.15 parts of hydrophobic agent.
[0037] Prepare as follows:
[0038] (1) Pre-mixing: Add 2 / 3 of water to the dispersion tank, add dispersant, anion additive and thickener, and mix at 400-800rpm for 5-10 minutes;
[0039] (2) Grinding and dispersing: Add seaweed mud at a speed of 1000-1500rpm, increase the speed to 2000-2500rpm and disperse for 5-10min, then reduce the speed to 1000-1500rpm, put in titanium dioxide, kaolin, mica p...
Embodiment 3
[0043] The net aldehyde antibacterial seaweed mud paint of the present embodiment comprises 18 parts of water, 0.5 part of dispersing agent, 0.8 part of antifreeze, 0.8 part of film-forming aid, 10 parts of titanium dioxide, 15 parts of calcium carbonate, 5 parts according to parts by weight. Kaolin, 2 parts of mica powder, 0.15 parts of nano-silver antibacterial agent, 3 parts of seaweed mud, 0.3 parts of thickener, 0.3 parts of negative ion additive, 15 parts of deodorant lotion, 0.15 parts of antifungal agent, 0.2 part of preservative and 0.1 part of hydrophobic agent.
[0044] Prepare as follows:
[0045] (1) Pre-mixing: add 2 / 3 of water to the dispersing tank, add dispersant, anion additive and thickener, mix at 400rpm for 10min;
[0046] (2) Grinding and dispersing: Add seaweed mud at a speed of 1000rpm, increase the speed to 2000rpm and disperse for 10min, then reduce the speed to 1000rpm, put in titanium dioxide, kaolin, mica powder and calcium carbonate, and disperse...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com