A technology of toner and fragrance type, which is applied in the field of toner preparation, can solve the problems of complex preparation method, high preparation cost, and large amount of essence used, and achieve the effects of low preparation cost, regular particle shape, and long-lasting fragrance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A kind of fragrant printing toner, the parts by weight of each component are:
[0022] 57 parts of magnetic iron oxide, 35 parts of styrene-acrylic resin, 23 parts of polypropylene wax, 13 parts of talcum powder, 3 parts of sodium silicate, and 0.25 parts of essence powder.
[0023] Its preparation method comprises the following steps:
[0024] Mix the magnetic iron oxide, polypropylene wax, talcum powder, sodium silicate, and essence powder, and ball mill for 40 minutes; add 80 parts by weight of deionized water, then add styrene-acrylic resin, and heat to 50°C. Hold for 50 minutes; wash with 4 times deionized water, filter and dry at 50°C to form granular materials; screen the materials, select 3-8 micron particles, and dry at 50°C for 30 minutes to obtain the product.
Embodiment 2
[0026] A kind of fragrant printing toner, the parts by weight of each component are:
[0027] 53 parts of magnetic iron oxide, 33 parts of styrene-acrylic resin, 20 parts of polypropylene wax, 10 parts of talcum powder, 1 part of sodium silicate, 0.1 part of essence powder.
[0028] Its preparation method comprises the following steps:
[0029] Mix the magnetic iron oxide, polypropylene wax, talcum powder, sodium silicate, flavor powder, and ball mill for 45 minutes; add 90 parts by weight of deionized water, then add styrene-acrylic resin, heat to 56 ° C, Hold for 55 minutes; wash with 6 times deionized water, filter and dry at 55°C to form granular materials; screen the materials, select particles of 3-8 microns, and dry at 55°C for 40 minutes to obtain the product.
Embodiment 3
[0031] A kind of fragrant printing toner, the parts by weight of each component are:
[0032] 55 parts of magnetic iron oxide, 33 parts of styrene-acrylic resin, 20 parts of polypropylene wax, 10 parts of talcum powder, 3 parts of sodium silicate, and 0.25 parts of essence powder.
[0033] Its preparation method comprises the following steps:
[0034] Mix the magnetic iron oxide, polypropylene wax, talcum powder, sodium silicate, flavor powder, and ball mill for 43 minutes; add 85 parts by weight of deionized water, then add styrene-acrylic resin, heat to 53 ° C, Hold for 53 minutes; wash with 5 times deionized water, filter and dry at 53°C to form granular materials; screen the materials, select 3-8 micron particles, and dry at 53°C for 35 minutes to obtain the product.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com