Improved external wall paint and preparation method thereof

A technology for exterior wall coatings and raw materials, applied in the field of improved exterior wall coatings and their preparation, to achieve the effects of excellent adhesion, fine texture and strong stain resistance

Inactive Publication Date: 2016-04-06
辛范范
View PDF9 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

Exterior wall latex paint not only needs good weather resistance and UV resistance, but also the coating film should be smooth and fine texture, but the existing exterior wall latex paint is difficult to meet the required requirements at the same time

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0013] The invention is an improved exterior wall paint, which is made of the following raw materials in parts by weight: 5 parts of attapulgite powder, 22 parts of white latex, 5 parts of titanium dioxide, 7.5 parts of deionized water, 6 parts of hydroxyethyl cellulose, 3.5 parts of trans-2-hexenal, 4.5 parts of styrene-ethylphenol polyoxyethylene ether, 1.2 parts of polyurethane modified nitrocellulose film-forming agent and 2.5 parts of dispersant. The dispersant is a low-molecular-weight ionomer in low-molecular-weight waxes.

[0014] A kind of preparation method of improved exterior wall paint, comprises the following steps:

[0015] 1) Weigh according to the formula, add attapulgite powder, deionized water and white latex into the mixer, and stir for 10 minutes at a speed of 600r / min;

[0016] 2) Then add hydroxyethyl cellulose and trans-2-hexenal, disperse and stir at a high speed of 1000r / min for 12min;

[0017] 3) Heat the mixture in the above steps to 60°C and keep...

Embodiment 2

[0020] The invention is an improved exterior wall paint, which is made of the following raw materials in parts by weight: 10 parts of attapulgite powder, 28 parts of white latex, 10 parts of titanium dioxide, 8.5 parts of deionized water, 12 parts of hydroxyethyl cellulose, 7.2 parts of trans-2-hexenal, 8.5 parts of styrene-ethylphenol polyoxyethylene ether, 13.5 parts of polyurethane modified nitrocellulose film-forming agent and 3.7 parts of dispersant.

[0021] A kind of preparation method of improved exterior wall paint, comprises the following steps:

[0022] 1) Weigh according to the formula, add attapulgite powder, deionized water and white latex into the mixer, and stir for 15 minutes at a speed of 700r / min;

[0023] 2) Then add hydroxyethylcellulose and trans-2-hexenal, disperse and stir at 1200r / min for 15min at high speed;

[0024] 3) Heat the mixture in the above steps to 70°C, keep it warm for 20 minutes, and then add phenethylphenol polyoxyethylene ether and pol...

Embodiment 3

[0027] The invention is an improved exterior wall paint, which is made of the following raw materials in parts by weight: 7 parts of attapulgite powder, 24 parts of white latex, 7 parts of titanium dioxide, 7.8 parts of deionized water, 9 parts of hydroxyethyl cellulose, 4.8 parts of trans-2-hexenal, 6.3 parts of styrene-ethylphenol polyoxyethylene ether, 2.6 parts of polyurethane modified nitrocellulose film-forming agent and 3.1 parts of dispersant.

[0028] A kind of preparation method of improved exterior wall paint, comprises the following steps:

[0029] 1) Weigh according to the formula, add attapulgite powder, deionized water and white latex into the mixer, and stir for 12 minutes at a speed of 650r / min;

[0030] 2) Then add hydroxyethyl cellulose and trans-2-hexenal, disperse and stir at a high speed of 1100r / min for 13min;

[0031] 3) Heat the mixture in the above steps to 65°C, keep it warm for 20 minutes, and then add phenethylphenol polyoxyethylene ether and poly...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
glossaaaaaaaaaa
adhesivityaaaaaaaaaa
Login to view more

Abstract

The invention discloses an improved external wall paint which is prepared from the following raw materials in parts by weight: 5-10 parts of attapulgite powder, 22-28 parts of white latex, 5-10 parts of titanium white, 7.5-8.5 parts of deionized water, 6-12 parts of hydroxyethyl cellulose, 3.5-7.2 parts of trans-2-hexenal, 4.5-8.5 parts of phenethyl phenol polyethenoxy ether, 1.2-3.5 parts of polyurethane modified nitrocellulose film former and 2.5-3.7 parts of dispersing agent. Compared with the existing latex paint, the external wall paint has the advantages of has the advantages of favorable weather resistance, favorable ultraviolet resistance and short drying time. After the hydroxyethyl cellulose and trans-2-hexenal are added, the coated film is flat and smooth, and has delicate tactile sensation. After the polyurethane modified nitrocellulose film former is added, the finished product has high fouling resistance and excellent adhesive force, can effectively prevent mildew and algae, has favorable leveling property, is safe and convenient for construction, and is an ideal external wall decorating material.

Description

Technical field [0001] The invention involves an improved exterior wall coatings and its preparation methods, which belongs to the field of architectural coatings. Background technique [0002] At present, there are many types of coatings used in exterior walls. Latex paint is one of the most widely used wall decorative materials, and latex paint is the most secure material among many coatings.The exterior wall latex paint not only requires good weather resistance, ultraviolet resistance, and the coating film should also be smooth and smooth, and the texture is delicate, while the existing existing lateral wall latex paint is difficult to meet the required requirements at the same time. Invention content [0003] In response to the lack of existing technology, the technical problem to be solved by the present invention is to provide an improved exterior wall coatings and their preparation methods, comprehensive performance, high weather resistance and ultraviolet resistance, and...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C09D131/04C09D101/28C09D7/12C09D5/16
CPCC09D131/04C08L2201/08C08L2205/035C09D5/16C09D7/61C09D7/63C08L1/284C08L71/02C08L1/18C08K3/346C08K2003/2241C08K5/07
Inventor 辛范范
Owner 辛范范
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products