A technology of offset printing ink and ink-based ink, which is applied in the field of offset printing ink and its preparation, can solve problems such as dispersibility, compatibility, poor fluidity, and poor dispersibility of wax paste, etc., so as to improve drying performance and Adsorption performance, excellent compatibility and fluidity, effect of improving compatibility and fluidity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0105] A kind of offset printing ink, its preparation steps are as follows (the following components are all calculated by weight percentage):
[0106] a. Prepare homemade quick-drying varnish:
[0107] a1. Put 15% semi-dry vegetable oil, 40% dry vegetable oil, 8% mineral oil, and 6% alkyd resin into the reaction kettle respectively, then raise the temperature to 60°C, and control the stirring speed to 300rpm, stirring for 5min;
[0108] a2. Slowly add 30% rosin-modified phenolic resin, raise the temperature to 200°C, control the stirring speed to 1000rpm, keep constant temperature and constant speed, and stir for 60min;
[0109] a3. Lower the temperature to 60-100°C, start to add 1% gelling agent, continue stirring for 60 minutes, and obtain self-made quick-drying varnish after stirring evenly;
[0110] b. Preparation of ink base ink:
[0111] Add 25% C.I. Pigment Yellow 12 filter cake pigment, 60% self-made quick-drying varnish, 6% calcium carbonate, 3% semi-dry vegetable ...
Embodiment 2
[0117] A kind of offset printing ink, its preparation steps are as follows (the following components are all calculated by weight percentage):
[0118] a. Prepare homemade quick-drying varnish:
[0119] a1. Put 11% semi-dry vegetable oil, 50% dry vegetable oil, 1% mineral oil, and 11% alkyd resin into the reaction kettle respectively, then raise the temperature to 65°C, and control the stirring speed to 250rpm, stirring for 10min;
[0120] a2. Slowly add 25% rosin-modified maleic acid resin, raise the temperature to 215°C, control the stirring speed to 800rpm, keep constant temperature and constant speed, and stir for 75min;
[0121] a3. Lower the temperature to 60-100°C, start to add 2% gelling agent, continue stirring for 70 minutes, and obtain self-made quick-drying varnish after stirring evenly;
[0122] b. Preparation of ink base ink:
[0123] Add 35% C.I. Pigment Red 57:1 filter cake pigment, 55% self-made quick-drying varnish, and 8% calcium carbonate to the kneader f...
Embodiment 3
[0129] A kind of offset printing ink, its preparation steps are as follows (the following components are all calculated by weight percentage):
[0130] a. Prepare homemade quick-drying varnish:
[0131] a1. Put 12% semi-dry vegetable oil, 35% dry vegetable oil, 4% mineral oil, and 8% alkyd resin into the reaction kettle respectively, then raise the temperature to 70°C, and control the stirring speed to 350rpm, and stir for 8 minutes;
[0132] a2. Slowly add 40% of the mixture made of rosin-modified phenolic resin and vegetable oil-modified alkyd resin in a weight ratio of 1:1, raise the temperature to 220°C, control the stirring speed to 1200rpm, and keep constant temperature and constant speed, stirring 50min;
[0133] a3. Lower the temperature to 60-100°C, start adding 1% gelling agent, continue to stir for 50 minutes, and obtain self-made quick-drying varnish after stirring evenly;
[0134] b. Preparation of ink base ink:
[0135] Add 20% C.I. Pigment Blue 15:3 filter cake...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com