[0030] A kind of concrete steps of the environmental protection dyeing method of jacquard denim are as follows:
[0031] (a) Weaving
[0032] The jacquard layer made of jute fiber and flax fiber is woven by ring spinning and the base layer made of bamboo charcoal fiber, paraben ester, cotton fiber and wool fiber is connected together by fabric heat-compression lamination process Form denim, wherein, the ratio of jute fiber and flax fiber is 3:2, bamboo charcoal fiber accounts for 22% of the mass percentage of bottom material layer, and described paraben accounts for 5% of the mass percentage of bottom material layer, cotton Fiber accounts for 50% of the mass percentage of bottom material layer, and wool fiber accounts for 15% of the mass percentage of bottom material layer;
[0033] (b) desizing
[0034] Add 1g of BF--7658 amylase, 2g of salt, 1g of penetrant and 0.5mL of glacial acetic acid to each liter of water to make a slurry. , arrange the denim in the slurry to fully...
Embodiment 2
[0050] A kind of environmental protection dyeing method concrete steps of jacquard denim are as follows:
[0051] (a) Weaving
[0052] The jacquard layer made of jute fiber and flax fiber is woven by ring spinning and the base layer made of bamboo charcoal fiber, paraben ester, cotton fiber and wool fiber is connected together by fabric heat-compression lamination process Form denim, wherein, the ratio of jute fiber and flax fiber is 3:1.5, and bamboo charcoal fiber accounts for 25% of the mass percentage of bottom material layer, and described paraben accounts for 6 of the mass percentage of bottom material layer, and cotton fiber Accounting for 55% of the mass percentage of the bottom material layer, wool fiber accounts for 18% of the mass percentage of the bottom material layer;
[0053] (b) desizing
[0054] Add 1.2g of BF--7658 amylase, 3g of salt, 1.2g of penetrant, 0.8mL of glacial acetic acid and 1g of softener to each liter of water to make a slurry. The pH value is...
Embodiment 3
[0070] A kind of concrete steps of the environmental protection dyeing method of jacquard denim are as follows:
[0071] (a) Weaving
[0072] The jacquard layer made of jute fiber and flax fiber is woven by ring spinning and the base layer made of bamboo charcoal fiber, paraben ester, cotton fiber and wool fiber is connected together by fabric heat-compression lamination process Form denim, wherein, the ratio of jute fiber and flax fiber is 3:2, and bamboo charcoal fiber accounts for 28 of the mass percent of bottom material layer, and described paraben accounts for 7 of the mass percent of bottom material layer, and cotton fiber accounts for 70% of the mass percentage of the bottom material layer wool fiber accounts for 20% of the mass percentage of the bottom material layer;
[0073] (b) desizing
[0074] Add 1.9g of BF-7658 amylase, 4.5g of salt, 1.8g of penetrant, 1.3mL of glacial acetic acid and 1.8g of softener to each liter of water to make a slurry. The pH value is 6...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com