Leather product zipper lubricating oil
A lubricating oil and zipper technology, applied in the field of leather goods processing, can solve problems such as difficult to pull, easy to rust, and affect the normal use of zippers, so as to prevent the deterioration of lubricating oil, prevent the chain teeth from rusting, and ensure normal use.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] (1) Add 10 parts of rice bran wax and 4 parts of hydrogenated castor oil to 15 parts of lanolin, heat to 80-90°C and mix for 10 minutes, then add 4 parts of fly ash, 3 parts of sepiolite powder and 1 part of nano glue powder, continue to heat to 110-120 ° C and mix for 5 minutes to obtain material I;
[0020] (2) Add 6 parts of vulcanized lard and 5 parts of film-forming aid to 10 parts of turpentine, mix well and let stand at 0-5°C for 1 hour, then add 4 parts of glyceryl behenate and 3 parts of Polyacrylamide, then heated to 70-80°C and mixed for 15 minutes to obtain material II;
[0021] (3) Add material II, 5 parts of microcrystalline cellulose, 3 parts of behenic acid amide, 2 parts of polyoxypropylene glyceryl ether and 1 part of monoglyceride laurate to material I, and grind to form a uniform paste.
[0022] Preparation of film-forming aids: first heat 15 parts of rosin pentaerythritol ester, 10 parts of rosin glyceride and 3 parts of rubber powder to 80-90 ° C ...
Embodiment 2
[0024] (1) Add 10 parts of rice bran wax and 2 parts of hydrogenated castor oil to 20 parts of lanolin, heat to 80-90°C and mix for 10 minutes, then add 6 parts of fly ash, 2 parts of sepiolite powder and 1 part of nano glue powder, continue to heat to 110-120 ° C and mix for 5 minutes to obtain material I;
[0025] (2) Add 6 parts of vulcanized lard and 3 parts of film-forming aids to 10 parts of turpentine, mix well and let stand at 0-5°C for 1 hour, then add 5 parts of glyceryl behenate and 3 parts of Polyacrylamide, then heated to 70-80°C and mixed for 15 minutes to obtain material II;
[0026] (3) Add material II, 8 parts of microcrystalline cellulose, 2 parts of behenic acid amide, 2 parts of polyoxypropylene glyceryl ether and 2 parts of monoglyceride laurate to material I, and grind to form a uniform paste.
[0027] Preparation of film-forming aids: First heat 12 parts of rosin pentaerythritol ester, 10 parts of rosin glyceride and 3 parts of rubber powder to 80-90 ° ...