Environment-friendly water-tolerant adhesive for wood
An adhesive and water-resistant technology, applied in the direction of adhesives, protein adhesives, polymer adhesive additives, etc., can solve the problems of poor water resistance of soybean adhesives, and the bonding strength cannot meet the production requirements of wood-based panels, etc., to achieve high bonding strength, Good water resistance and broad market prospects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0017] Embodiment 1: a kind of adhesive for environment-friendly water-resistant type wood, its preparation method is:
[0018] (1) Dissolve 26 parts of low-temperature defatted soybean powder in 120 parts of water, stir evenly at 35°C, adjust the pH to 5.0, add 12 parts of sodium lauryl sulfate and 2.0 parts of sodium humate, and keep it at 35°C for 4 hours to obtain Soybean flour slurry after pretreatment;
[0019] (2) Adjust the pH of the pretreated soybean flour slurry to 11.0, add 0.2 parts of glutaraldehyde and react at 30°C for 1 hour, raise the temperature to 45°C, add 0.3 parts of carboxymethylcellulose sodium, and react for 75 minutes to obtain a semi-finished adhesive;
[0020] (3) Add 3.8 parts of herbal extracts to the semi-finished adhesive, raise the temperature to 55°C, stir at 150r / min for 5h, then cool to room temperature to obtain the product.
[0021] The preparation method of the herbal extract is as follows: 3 parts of cinnamon, 12 parts of Imperata rhiz...
Embodiment 2
[0022] Embodiment 2: a kind of adhesive for environment-friendly water-resistant type wood, its preparation method is:
[0023] (1) Dissolve 26 parts of low-temperature defatted soybean powder in 120 parts of water, stir evenly at 35°C, adjust the pH to 5.0, add 12 parts of sodium lauryl sulfate and 1.5 parts of sodium humate, and keep it at 35°C for 4 hours to obtain Soybean flour slurry after pretreatment;
[0024] (2) Adjust the pH of the pretreated soybean flour slurry to 11.0, add 0.2 parts of glutaraldehyde and react at 30°C for 1 hour, raise the temperature to 40°C, add 0.1 part of sodium carboxymethylcellulose, and react for 70 minutes to obtain a semi-finished adhesive;
[0025] (3) Add 3.2 parts of herbal extracts to the semi-finished adhesive, heat up to 50°C, stir at 100r / min for 3h, then cool to room temperature to obtain the product.
[0026] The preparation method of the herbal extract is as follows: 1 part of cassia bark, 10 parts of Imperata praecox root, 6 p...
Embodiment 3
[0027] Embodiment 3: a kind of adhesive for environment-friendly water-resistant type wood, its preparation method is:
[0028] (1) Dissolve 26 parts of low-temperature defatted soybean powder in 120 parts of water, stir evenly at 35°C, adjust the pH to 5.0, add 12 parts of sodium lauryl sulfate and 2.5 parts of sodium humate, and keep it at 35°C for 4 hours to obtain Soybean flour slurry after pretreatment;
[0029] (2) Adjust the pH of the pretreated soybean flour slurry to 11.0, add 0.2 parts of glutaraldehyde and react at 30°C for 1 hour, raise the temperature to 50°C, add 0.5 parts of carboxymethylcellulose sodium, and react for 80 minutes to obtain a semi-finished adhesive;
[0030] (3) Add 4.5 parts of herbal extract to the semi-finished adhesive, heat up to 60°C, stir at 200r / min for 6h, then cool to room temperature to obtain the product.
[0031] The preparation method of the herbal extract is as follows: 5 parts of cassia bark, 15 parts of coriander root, 10 parts ...