A kind of preparation method of antifouling sofa fabric
A sofa and fabric technology, applied in the direction of repelling fibers, physical treatment, yarn, etc. to liquids, can solve the problems of weak anti-fouling ability, easy to appear stains on the sofa surface, etc., to prevent oil spots, good anti-mildew effect, improve the effect of strength
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] A preparation method for an antifouling sofa fabric, comprising the following steps:
[0025] (1) Prepare the fibers required for the sofa fabric, including 50 g of flax fiber, 30 g of polyurethane fiber, 80 g of polyester fiber, and 60 g of graphite fiber, in which the diameter of the polyester fiber is three times the diameter of the graphite fiber;
[0026] (2) Soak the polyester fibers in 0.3 mol / L sodium hydroxide solution and irradiate with microwaves. The soaking temperature is 45-55°C, the soaking time is 60 minutes, and the radiation starts after 30 minutes of soaking. The irradiation time is 10 minutes, and the radiation power 50W, after taking it out, wash it with deionized water and ventilate and dry;
[0027] (3) Add 0.5 g / mL of nano-silica, 0.08 g / mL of ultrafine powder of fluorine-containing silicon polymer particles, 0.02 g / mL of poly-N-isopropylacrylamide, and 0.02 g of shellac to the sodium hydroxide solution / mL, stir well and mix uniformly to obtain...
Embodiment 2
[0033] A preparation method for an antifouling sofa fabric, comprising the following steps:
[0034] (1) Prepare the fibers required for the sofa fabric, including 55 g of flax fiber, 35 g of polyurethane fiber, 90 g of polyester fiber, and 70 g of graphite fiber in the following parts by weight, wherein the diameter of the polyester fiber is the diameter of the graphite fiber 4 times of
[0035] (2) Soak the polyester fiber in 0.4 mol / L sodium hydroxide solution and add microwave radiation. The soaking temperature is 50°C, the soaking time is 60 minutes, and the radiation starts after 30 minutes of soaking. The irradiation time is 12 minutes, and the radiation power is 60 W, after taking it out, wash it with deionized water and ventilate and dry;
[0036] (3) Preparation of impregnation solution: Add 0.65 g / mL of nano-silica, 0.10 g / mL of ultrafine powder of fluorine-containing silicon polymer particles, 0.03 g / mL of poly-N-isopropylacrylamide, Shellac 0.03 g / mL, stir well ...
Embodiment 3
[0042] A preparation method for an antifouling sofa fabric, comprising the following steps:
[0043] (1) Prepare the fibers required for the sofa fabric, including 60 g of flax fiber, 40 g of polyurethane fiber, 100 g of polyester fiber, and 80 g of graphite fiber in the following parts by weight, wherein the diameter of the polyester fiber is the diameter of the graphite fiber 5 times;
[0044] (2) Soak the polyester fiber in 0.5 mol / L sodium hydroxide solution and add microwave radiation. The soaking temperature is 55°C, the soaking time is 60 minutes, and the radiation starts after 30 minutes of soaking. The irradiation time is 15 minutes, and the radiation power is 70 W, after taking it out, wash it with deionized water and ventilate and dry;
[0045] (3) Preparation of impregnation solution: Add 0.8 g / mL of nano-silica, 0.12 g / mL of fluorine-containing silicon polymer particle ultrafine powder, 0.04 g / mL of poly-N-isopropylacrylamide, Shellac 0.04 g / mL, stir well and mi...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com