Weak-solvent ink for spinning ink jet and preparation method thereof
A weak solvent, inkjet technology, applied in the field of ink, can solve the problem that the picture cannot be used outdoors, and achieve the effect of bright colors, good inkjet continuity and high stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0038] Disperse Red 60: 10%
[0039] Alkylphenol polyoxyethylene ether condensate: 5%;
[0040] Alcohol-soluble acrylic resin S-70: 10%;
[0041] Division 80: 2%;
[0042] Leveling agent: 2%
[0043] Defoamer: 4%
[0044] Anti-sedimentation agent: 4%
[0045] Diethylene glycol ether: 63%
[0046] Dissolve the resin linker, dispersant, surfactant, and other additives in the solvent according to the formula, stir evenly, then add organic disperse dyes, and stir at a high speed for 30 minutes at a stirring speed of 1000r / min to form a pre-dispersion. Then the pre-dispersed liquid is transferred to a ball mill, ball milled for 4 hours, and the obtained dispersion liquid is filtered with a 500nm microporous membrane, filled and packaged to obtain a weak solvent red ink for textile inkjet, wherein the viscosity is 6.5mpa.s, the surface The tension is 34.2mN / m, and the pH is 7.2. The red ink has good inkjet continuity and bright colors.
Embodiment 2
[0048] Disperse Blue 56: 20%
[0049] Polyol polyoxyethylene ether: 10%;
[0050] Alcohol-soluble acrylic resin S-70:5%;
[0051] Division 80: 2.5%;
[0052] Leveling agent: 0.5%
[0053] Defoamer: 1%
[0054] Anti-sedimentation agent: 1%
[0055] Diethylene glycol ether: 60%
[0056] Dissolve the resin linker, dispersant, surfactant, and other additives in the solvent according to the formula, stir evenly, then add organic disperse dyes, and stir at a high speed for 60 minutes at a stirring rate of 1000r / min to form a pre-dispersion. Then the pre-dispersion is transferred to a ball mill, ball milled for 8 hours, the resulting dispersion is filtered with a 800nm microporous membrane, filled and packaged to obtain a weak solvent blue ink for textile inkjet, wherein the viscosity is 7.2mpa.s, The surface tension is 33.4mN / m, and the pH is 7.1. The blue ink has good inkjet continuity and bright colors.
Embodiment 3
[0058] Disperse Yellow 64: 5%
[0059] Acrylate hyperdispersant: 2%;
[0060] Alcohol-soluble acrylic resin S-70: 20%;
[0061] Ethylene glycol: 5%;
[0062] Leveling agent: 0.2%
[0063] Defoamer: 0.4%
[0064] Anti-sedimentation agent: 0.4%
[0065] Ethylene glycol butyl ether acetate: 67%
[0066] Dissolve the resin linker, dispersant, surfactant, and other additives in the solvent according to the formula, stir evenly, then add organic disperse dyes, and stir at a high speed for 60 minutes at a stirring speed of 800r / min to form a pre-dispersion. Then the pre-dispersion is transferred to a ball mill, ball milled for 2 hours, the resulting dispersion is filtered with a 400nm microporous membrane, filled and packaged to obtain a weak solvent blue ink for textile inkjet, wherein the viscosity is 12.8mpa.s, The surface tension is 33.8mN / m, and the pH is 6.8. The yellow ink has good inkjet continuity and bright colors.
PUM
| Property | Measurement | Unit |
|---|---|---|
| viscosity | aaaaa | aaaaa |
| surface tension | aaaaa | aaaaa |
| viscosity | aaaaa | aaaaa |