A kind of environment-friendly, high-hiding yellow color paste, preparation method and application thereof
A kind of yellow color paste, environment-friendly technology, applied in the direction of pigment paste, coating, polyester coating, etc., can solve the problems of water, soil heavy metal pollution, low transparency of yellow color paste, great harm to consumers, etc., reaching the factory The effect of low equipment requirements, high chroma, and high weather resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0049]According to the method of the present invention, adopt raw materials as shown in table 1 to prepare environment-friendly, high hiding power yellow color paste:
[0050] Table 1
[0051]
[0052]
[0053] The preparation method comprises the following steps:
[0054] Step 1: Premix
[0055] A. Put 13.74 parts of R-5534 alkyd resin and 1 part of S-100# solvent oil into the production tank, then start stirring, and continue to put in 0.72 parts of EFKA-4401 dispersion aid and 12 parts of pigment DCC YELLOW 5RLX in sequence;
[0056] B. Stop stirring after the feeding is completed, and clean the cylinder wall and stirring shaft with 0.5 parts of S-100# solvent oil;
[0057] C. Start stirring again, and stir at a high speed of 1000-1200 rpm for 30 minutes to obtain a mixture.
[0058] Step Two: Sanding
[0059] A. Sand grind the mixture obtained in the first step to a fineness of ≤5 μm, filter out the sand and grind it into cylinder A, clean the sand mill with 1 pa...
Embodiment 2
[0077] According to the method of the present invention, adopt raw materials as shown in table 3 to prepare environment-friendly, high hiding power yellow color paste:
[0078] table 3
[0079]
[0080]
[0081] The preparation method comprises the following steps:
[0082] Step 1: Premix
[0083] A. Put 12 parts of R-5534 alkyd resin and 0.6 parts of S-100# solvent oil into the production tank, then start stirring, and continue to put in 0.4 parts of EFKA-4401 dispersion aid and 8.02 parts of pigment DCC YELLOW 5RLX in sequence;
[0084] B. Stop stirring after the feeding is completed, and clean the cylinder wall and stirring shaft with 0.5 parts of S-100# solvent oil;
[0085] C. Start stirring again, and stir at a high speed of 1000-1200 rpm for 30 minutes to obtain a mixture.
[0086] Step Two: Sanding
[0087] A. Sand grind the mixture obtained in the first step to a fineness of ≤5 μm, filter out the sand and grind it into cylinder A, clean the sand mill with 0....
Embodiment 3
[0106] According to the method of the present invention, adopt raw materials as shown in table 5 to prepare environment-friendly, high hiding power yellow color paste:
[0107] table 5
[0108] serial number Component parts by weight 1 R-5534 alkyd resin 15 copies 2 S-100# solvent oil 1.5 servings 3 EFKA-4401 Dispersant 1 copy 4 Pigment DCC YELLOW 5RLX 16.77 copies 5 S-100# solvent oil 2 copies 6 S-100# solvent oil 4 parts 7 R-5534 alkyd resin 20 copies 8 R-4150 alkyd resin 15.5 servings 9 R-1327 alkyd resin 19.1 copies 10 UVAN 128 amino resin 28.5 servings 11 DISPARLON KS-281 dispersing aid 0.5 parts 12 Butanol 3.6 servings
[0109] The preparation method comprises the following steps:
[0110] Step 1: Premix
[0111] A. Put 15 parts of R-5534 alkyd resin and 1.5 parts of S-100# solvent oil into the production tank, then start stirring, and continue to put in 1 p...