Embodiment 1
[0015] A method for waxing willow furniture, specifically the following steps:
[0016] (1) Soak willow in concentrated brine
[0017] Soak willow wood, the raw material for willow furniture, in concentrated brine for 50-60 minutes. During the soaking period, heat slowly until it boils and then keep warm at 70-80°C. Rinse well; the concentrated brine is prepared by mixing 100 parts of water, 5 parts of sodium chloride, 0.5 parts of copper sulfate, 0.1 part of ferric chloride, 1 part of menthol, and 30 parts of plant extracts in parts by mass ;
[0018] (2) Willow waxing
[0019] Dry the treated willow wood until the moisture content is below 2%, then apply wax oil evenly on the surface of the willow wood, wrap it with a film, and place it in the warehouse for 8-12 hours, then remove the film, wipe it with a cotton cloth, and wipe it after finishing Place in an oven at 60-70°C and heat-preserve for 30-40 minutes; the wax oil, in parts by mass, consists of 5 parts of turpenti...
Embodiment 2
[0023] A method for waxing willow furniture, specifically the following steps:
[0024] (1) Soak willow in concentrated brine
[0025] Soak willow wood, the raw material for willow furniture, in concentrated brine for 50-60 minutes. During the soaking period, heat slowly until it boils and then keep warm at 70-80°C. Rinse well; the concentrated brine is prepared by mixing 120 parts of water, 10 parts of sodium chloride, 1 part of copper sulfate, 0.2 parts of ferric chloride, 2 parts of menthol, and 40 parts of plant extracts in parts by mass. ;
[0026] (2) Willow waxing
[0027] Dry the treated willow wood until the moisture content is below 2%, then apply wax oil evenly on the surface of the willow wood, wrap it with a film, and place it in the warehouse for 8-12 hours, then remove the film, wipe it with a cotton cloth, and wipe it after finishing Place in an oven and bake at 60-70°C for 30-40 minutes; the wax oil, in parts by mass, consists of 8 parts of turpentine, 3 pa...
Embodiment 3
[0031] A method for waxing willow furniture, specifically the following steps:
[0032] (1) Soak willow in concentrated brine
[0033] Soak willow wood, the raw material for willow furniture, in concentrated brine for 50-60 minutes. During the soaking period, heat slowly until it boils and then keep warm at 70-80°C. Rinse well; the concentrated brine is prepared by mixing 110 parts of water, 8 parts of sodium chloride, 0.7 parts of copper sulfate, 0.15 parts of ferric chloride, 1.5 parts of menthol, and 35 parts of plant extracts in parts by mass ;
[0034] (2) Willow waxing
[0035] Dry the treated willow wood until the moisture content is below 2%, then apply wax oil evenly on the surface of the willow wood, wrap it with a film, and place it in the warehouse for 8-12 hours, then remove the film, wipe it with a cotton cloth, and wipe it after finishing Place in an oven at 60-70°C and heat-preserve for 30-40 minutes; the wax oil, in parts by mass, consists of 6 parts of tur...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com