Novel environment-friendly waterproof and oil-proof paper and preparation method thereof
An oil-proof paper and environmental protection technology, applied in the field of paper, paper and paper manufacturing, can solve the problems of human harm, limited popularization and application, poor mechanical properties, etc., and achieve easy operation, high degree of recyclability, and human safety high effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] The new environment-friendly waterproof and oil-proof paper includes ordinary paper layer and coating layer. The coating layer is evenly coated on the upper and lower sides of the ordinary paper layer. The coating layer is composed of the following ingredients in weight percentage: anion modified starch 5%, chitosan 2%, fluorine Plain paper oil repellant 1.2%, alkyl ketene dimer 0.8%, tap water 91%
[0023] The preparation method of the new environment-friendly waterproof and oil-proof paper, the preparation method includes the following steps: the first step is to disperse the anionic modified starch into water, and perform ultrasonic oscillation in an ultrasonic cleaning machine, control the ultrasonic power to 2000W, and the frequency to 800HZ, and vibrate The time is 5min, disperse evenly, the homogeneous aqueous solution that forms; The second step, under the mechanical stirring condition that stirring speed is 800r / min, add chitosan, fluorine paper product oil repe...
Embodiment 2
[0025] Take 8% of anionic modified starch, 1% of polyamide polyepichlorohydrin resin, 1% of fluorine paper oil repellent and fluorocarbon water and oil repellent (mass ratio 1:1), 1% of carboxymethyl cellulose and tap water 89%.
[0026] Disperse the anion-modified starch into water, perform ultrasonic oscillation in an ultrasonic cleaning machine, control the ultrasonic power to 2000W, the frequency to 1000HZ, and the oscillation time to 10min, disperse evenly, and form a uniform aqueous solution, then, at a stirring speed of 1500r / Under the condition of mechanical stirring for min, add polyamide polyepichlorohydrin resin, fluorine paper oil repellent, fluorocarbon water and oil repellent (mass ratio 1:1) and carboxymethyl cellulose, and keep the above ultrasonic conditions for oscillation 15min, heating 85 o Stir for 3.5 h under the condition of C to obtain a waterproof and oil-repellent coating; then, evenly coat the prepared waterproof and oil-proof coating on both sides...
Embodiment 3
[0028] Take 5% cationic modified starch, 3% chitosan and polyethyleneimine (mass ratio 1:1), 2% fluorocarbon water and oil repellent, 5% carboxymethyl cellulose and 85% tap water.
[0029] Disperse cationic modified starch into water, perform ultrasonic oscillation in an ultrasonic cleaning machine, control the ultrasonic power to 2000W, frequency to 800HZ, oscillation time to 15min, disperse evenly, and form a homogeneous aqueous solution, then, at a stirring speed of 500r / Under the condition of mechanical stirring for 1 min, add chitosan and polyethyleneimine (mass ratio 1:1), fluorocarbon water and oil repellent and carboxymethyl cellulose, maintain the above ultrasonic conditions for 15 min, and heat for 90 min. o Stir for 3.5 h under the condition of C to obtain a waterproof and oil-repellent coating; then, evenly coat the prepared waterproof and oil-proof coating on both sides of the paper, place the coated paper in an oven at a temperature of 100 o Under C, dry for 10 ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com