Long-acting slump prevention agent and preparation method thereof
A slump retaining agent and long-acting technology, which is applied in the field of long-acting slump retaining agent and its preparation, can solve the problems of inconvenient long-distance and long-term transportation, the inability to pour out concrete, and reduce the capacity of tank trucks, etc., to achieve high strength, low bleeding, and The effect of reducing the chance of impurity formation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0025] 1. Add 1350 kg of water into the 5000L reactor, then add 1700 kg of imported ether and start stirring to dissolve the ether. During the dissolution process, the temperature of the reactor is raised to 58°C±2°C, and nitrogen gas is introduced after the temperature stabilizes (to produce polycondensation Reaction makes reaction more fully) after slowly adding 17 kilograms of B2 powder (sodium methacryl sulfonate) and continuing to stir for 5 minutes, then slowly adding 6.8 kilograms of ammonium peroxide, the reaction kettle is always in stirring state in the whole reaction process.
[0026] 2. Prepare materials A and B,
[0027] Material A is prepared by stirring 2.9 kg of imported AC (thioglycolic acid) and 300 kg of water.
[0028] Material B is prepared by stirring 222 kg of A2 liquid (strong ethyl ester), 80 kg of acrylic acid and 120 kg of water.
[0029] In order to ensure the reaction effect, both material A and material B are prepared 15 minutes before the dropwi...
Embodiment 2
[0035] 1. Add 1350 kg of water into the 5000L reactor, then add 1785 kg of imported ether and start stirring to dissolve the ether. During the dissolution process, the temperature of the reactor is raised to 58°C±2°C, and nitrogen gas is introduced after the temperature is stable (to produce polycondensation Reaction makes reaction more fully) after slowly adding 17 kilograms of B2 powder (sodium methacrylic sulfonate) and continue to stir for 5 minutes, then slowly add 6.5 kilograms of ammonium peroxide, and the reaction kettle is always in stirring state in the whole reaction process.
[0036] 2. Prepare materials A and B,
[0037] Material A is prepared by stirring 2.5 kg of imported AC (thioglycolic acid) and 300 kg of water.
[0038] Material B is prepared by stirring 210 kg of A2 liquid (strong ethyl ester), 80 kg of acrylic acid and 120 kg of water.
[0039] In order to ensure the reaction effect, both material A and material B are prepared 15 minutes before the dropwi...
Embodiment 3
[0045] 1. Add 1350 kg of water into the 5000L reactor, then add 1700 kg of imported ether and start stirring to dissolve the ether. During the dissolution process, the temperature of the reactor is raised to 58°C±2°C, and nitrogen gas is introduced after the temperature stabilizes (to produce polycondensation Reaction makes reaction more fully) after slowly adding 17 kilograms of B2 powder (sodium methacryl sulfonate) and continuing to stir for 5 minutes, then slowly adding 7 kilograms of ammonium peroxide, the reaction kettle is always in stirring state in the whole reaction process.
[0046] 2. Prepare materials A and B,
[0047] Material A is prepared by stirring 2.9 kg of imported AC (thioglycolic acid) and 300 kg of water.
[0048] Material B is prepared by stirring 222 kg of A2 liquid (strong ethyl ester), 80 kg of acrylic acid and 120 kg of water.
[0049] In order to ensure the reaction effect, both material A and material B are prepared 15 minutes before the dropwise...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com